Long-Lived Na–CO2 Batteries
October 9, 2024 – Sodium–carbon dioxide batteries could store renewable electricity while recycling CO2, but so far they have not lasted long. Researchers from the Technical University of Ilmenau, Ulm University and Zhengzhou University have now developed a “two-in-one” electrode with defects on several length scales that serves as both the sodium anode host and the CO2 cathode. As a cathode, it ran for about 2400 cycles (4800 hours), longer than any cathode reported for Na–CO2 batteries before.
A battery that breathes in carbon dioxide sounds like a good deal: sodium–carbon dioxide (Na–CO2) batteries run on the reaction 4Na + 3CO2 ↔ 2Na2CO3 + C, reach a high energy density of 1125 Wh kg−1, and could recycle the greenhouse gas CO2 while storing electricity from renewable sources.1 Their weak point is a short life.1–3 On the cathode side, the catalyst is often too weak to break down the inert discharge product sodium carbonate (Na2CO3) completely. The carbonate piles up, clogs the pores through which Na+ ions and CO2 travel, and passivates the active surface.4–6 On the anode side, the highly reactive sodium metal is dissolved and deposited again in every cycle. This causes large volume changes, needle-like dendrites and inactive “dead” sodium, which can make the battery fail early.7–9 Extra sodium foil is often added to make up for the losses, but it works against the intended application and does nothing against dendrites.10,11
Many strategies target one electrode at a time. Cathodes are made by spraying a catalyst onto a conductive carbon gas diffusion layer.12,13 Anodes are stabilized with tailored electrolytes,11 a stable NaF-rich interphase,14 sodium-containing composite anodes3 or solid-state electrolytes.7,8 Such one-sided solutions cannot solve the problems of the battery as a whole, the researchers argued; anode and cathode should be designed together. For Na–CO2 batteries, such a joint design had not yet led to a breakthrough.
A New Electrode Design for Na–CO2 Batteries
The team’s answer is a single electrode that does both jobs (Fig. 1a): a porous 3D carbon paper (CP) covered with copper-doped iron oxide nanoparticles, called CP@FeCu. As an anode host, it should attract sodium (be “sodiophilic”) and let it nucleate easily and evenly. As a cathode, it should catalyse both the CO2 reduction reaction during discharge (CO2RR) and the CO2 evolution reaction during charge (CO2ER). The key is what materials scientists call atomic size misfit: when atoms of different sizes are forced into one lattice, they create lattice distortions, dislocations and interfacial defects.15–20 These defects change the stress in the lattice and the surface charge of the electrode, and with it both sodium deposition and CO2 conversion.
Density-functional theory (DFT) calculations first tested the idea on a simplified model, an Fe3O4 cluster with a single copper atom on carbon, compared with the copper-free CP@Fe and bare CP. Copper doping redistributed the charge and moved electrons from the iron oxide cluster into the carbon, a sign of strong coupling at the CP@FeCu interface (Figs. 1b, c). It also raised the d-band centre, a widely used measure of how strongly a metal binds adsorbates,21 from −2.4213 to −2.2557 eV (Fig. 1d). Accordingly, sodium bound much more strongly to CP@FeCu (−3.27 eV) than to CP@Fe (−2.30 eV) or bare carbon paper (−0.83 eV), and CO2 also adsorbed best on CP@FeCu (Fig. 1e). The calculations further showed that the copper-doped interface stretches and weakens the Na–O bonds in Na2CO3, which should make the discharge product easier to decompose on charging.
Defects Seen Atom by Atom
The electrodes were made from copper–iron Prussian blue analogue nanocubes grown on the carbon paper and then heat-treated; CP@Fe was made the same way without copper salts. To see which defects actually form, the team imaged CP@FeCu with the CC/CS-corrected SALVE microscope at Ulm University at 80 kV.22 The HRTEM images show densely packed nanoparticles with nanometre-sized grains and many grain boundaries (Figs. 2a, h). Region I in Fig. 2a is a twinned copper nanoparticle with lattice fringes 0.209 nm apart, matching the (111) planes of copper. An intensity profile along a row of copper atoms reveals gaps where atoms are missing (Figs. 2b, c). Region II shows fringes 0.243 nm apart, the (222) planes of Fe3O4 (Fig. 2e). Other particles are twinned with a spacing of 0.235 nm, which fits the (222) planes of CuO or Fe3O4 (Fig. 2i), and some are single-crystal copper with a Cu–Cu distance of 2.29 Å (Fig. 2l).
Filtered images, obtained by inverse fast Fourier transformation (IFFT), reveal strongly disordered lattice planes with edge dislocations (Figs. 2d, f, j, k). Geometric phase analysis, which turns small shifts of lattice fringes into a strain map, shows that the shear strain concentrates along the grain boundaries and defects (Figs. 2g, n). Electron diffraction confirms that the particles contain both Fe3O4 and copper (Fig. 2m), and element maps show iron and copper evenly distributed, mixed with nitrogen and carbon (Fig. 2o). In the copper-free CP@Fe, by contrast, the lattice is regular throughout the particles. The researchers therefore describe CP@FeCu as an electrode with “multiscale defective interfaces”: atomic copper defects, twin boundaries, nanoscale mosaic grains, vacancies and lattice distortions.
A Stable Sodium Anode
As an anode host, CP@FeCu let sodium be plated and stripped for about 3960 hours, while bare copper foil short-circuited after 460 hours (Fig. 3a). That is 1980 cycles with an average Coulombic efficiency, the share of the plated sodium that is recovered on stripping, of about 99.1% (Fig. 3b). This clearly exceeds hosts with sodiophilic coatings,23–32 carbon skeletons33–38 or metal scaffolds39,40 (Fig. 3h). The box below explains how the sodium grows on the three hosts; Fig. 4 with the microscopy images is inside the box.
A Durable CO2 Cathode
Next, CP@FeCu served on its own as the cathode of a Na–CO2 battery, with CP@Fe as a control and 1 M NaClO4 in TEGDME as a less volatile electrolyte. Cyclic voltammetry (CV) between 1.8 and 4.2 V at 0.1 mV s−1 showed the CO2RR at about 2.3 V and the CO2ER at about 4 V (Fig. 5a). Only CP@FeCu showed additional peaks at about 3.17 and 3.70 V, which the researchers attributed to iron and copper switching between oxidation states (Fe0/Fe2+/Fe3+ and Cu0/Cu2+). Such valence oscillations help both CO2 reduction and CO2 evolution and thus lower the overpotential of the battery.44–46 The gap between charge and discharge voltage was 1.55 V with CP@FeCu, compared with 2.0 V with CP@Fe (Fig. 5b).
In cycles of two hours each at 10 µA cm−2, the CP@Fe cathode lasted about 450 hours, or 210 cycles (Fig. 5c). With too few active sites, Na2CO3 was not fully converted back on charging. The insulating carbonate accumulated, blocked the transport of Na+ and CO2, raised the polarization and finally killed the battery. CP@FeCu tripled the cycle life to 600 stable cycles. At 5 µA cm−2, it ran for 2400 cycles (4800 hours) with a discharge voltage of 2.2 V (Fig. 5d), clearly longer than all earlier Na–CO2 cathodes (Fig. 5e).2,3,4,5,7,8,10,11,12,13,14,47,48,49,50,51,52 The battery also cycled stably at 50 and 100 µA cm−2. In the first cycles, the charging curve showed two plateaus, caused by the changing oxidation states of iron and copper; after repeated cycling, these settled into a stable configuration and only one plateau remained.
Ex situ measurements confirmed that the reaction is reversible. After discharge, X-ray diffraction and Raman spectra showed new peaks of crystalline Na2CO3, which disappeared after charging (Figs. 5f, g). TEM images showed the cathode densely covered with product after discharge and clean again after charging, and electron diffraction found Na2CO3 only in the discharged state (Figs. 5h–k). In scanning electron micrographs, Na2CO3 covered the whole carbon fibre surface after discharge, and the fibres reappeared after charging (Figs. 5l, m).
Why the Defects Help
HRTEM images of the electrode after discharge and after charging show that the defects survive (Figs. 6e, f). The interconnected nanoparticles still consist of many crystalline and amorphous nanodomains with grain boundaries, copper atom defects, edge dislocations and distorted atomic rows. In copper-rich regions, copper atoms even extend into the lattice of neighbouring Fe3O4 grains. According to the researchers, such distortions make it easier for electrons to move between iron and copper and for their oxidation states to change, which drives the catalysis. That the defect structures are preserved after cycling explains the long life of the electrode. X-ray photoelectron spectroscopy and DFT calculations show how the oxidation states change and why the reactions run more easily on CP@FeCu; the box below gives the details.
Towards Anode-Less Batteries
As a proof of concept, the team built a full cell in which CP@FeCu serves on both sides: loaded with 50 mAh cm−2 of sodium as the anode, and bare as the cathode (CP@FeCu-Na||CP@FeCu, Fig. 7a). The sodium-loaded electrode was dense and smooth and only about 0.45 mm thick, while the same amount of sodium on copper foil formed an uneven surface with dendrites (Figs. 7b, c). The terminal discharge voltage of the CP@FeCu cell stayed above 2 V after 100 cycles, whereas a cell with sodium on copper (Cu-Na||CP@FeCu) declined after only 20 cycles (Fig. 7d). The CP@FeCu cell ran for more than 240 cycles (480 hours) at 5 µA cm−2 and more than 100 cycles (200 hours) at 10 µA cm−2 with almost unchanged charge and discharge curves (Fig. 7e).
The work shows that defects are not just flaws: introduced deliberately on several length scales, they can make one electrode serve both sides of a Na–CO2 battery. Atomic-resolution imaging at Ulm University made the copper defects, dislocations and strained grain boundaries visible, and showed that they survive thousands of hours of cycling. Even in an open system such as a Na–CO2 cell, a small amount of sodium can then greatly extend battery life, which could help future anode-less and anode-free sodium metal batteries, not only Na–CO2 batteries. The findings “may shed new light on the systematic design of ‘two-in-one’ electrodes based on the superiority of multiscale defective interfaces for energy conversion and storage fields and beyond,” the authors conclude.
Resource:
Xu, C., Hong, P., Dong, Y., Li, Y., Shen, Y., Biskupek, J., Zhao, H., Kaiser, U., Shao, G. & Lei, Y. (2024).
Multiscale defective interfaces for realizing Na–CO2 batteries with ultralong lifespan.
Adv. Mater., 36(48), 2409533.
https://doi.org/10.1002/adma.202409533
Download this news article as PDF – for reading on paper, taking notes or filing.
-
Xu, C., Dong, Y., Shen, Y., et al. (2023). Fundamental Understanding of Nonaqueous and Hybrid Na–CO2 Batteries: Challenges and Perspectives. Small, 19, 2206445. https://doi.org/10.1002/smll.202206445
-
Hu, X., Sun, J., Li, Z., et al. (2016). Rechargeable Room‐Temperature Na–CO2 Batteries. Angewandte Chemie International Edition, 55, 6482–6486. https://doi.org/10.1002/anie.201602504
-
Hu, X., Li, Z., Zhao, Y., et al. (2017). Quasi–solid state rechargeable Na-CO2 batteries with reduced graphene oxide Na anodes. Science Advances, 3, e1602396. https://doi.org/10.1126/sciadv.1602396
-
Pichaimuthu, K., Jena, A., Chang, H., et al. (2022). Molybdenum Disulfide/Tin Disulfide Ultrathin Nanosheets as Cathodes for Sodium–Carbon Dioxide Batteries. ACS Applied Materials & Interfaces, 14, 5834–5842. https://doi.org/10.1021/acsami.1c22435
-
Fang, C., Luo, J., Jin, C., et al. (2018). Enhancing Catalyzed Decomposition of Na2CO3 with Co2MnOx Nanowire-Decorated Carbon Fibers for Advanced Na–CO2 Batteries. ACS Applied Materials & Interfaces, 10, 17240–17248. https://doi.org/10.1021/acsami.8b04034
-
Yang, X., Zhang, D., Zhao, L., et al. (2024). Upgrading Cycling Stability and Capability of Hybrid Na‐CO2 Batteries via Tailoring Reaction Environment for Efficient Conversion CO2 to HCOOH. Advanced Energy Materials, 14, 2304365. https://doi.org/10.1002/aenm.202304365
-
Mao, Y., Chen, X., Cheng, H., et al. (2022). Forging Inspired Processing of Sodium‐Fluorinated Graphene Composite as Dendrite‐Free Anode for Long‐Life Na–CO2 Cells. Energy & Environmental Materials, 5, 572–581. https://doi.org/10.1002/eem2.12191
-
Lu, L., Sun, C., Hao, J., et al. (2023). A High‐Performance Solid‐State Na–CO2 Battery with Poly(Vinylidene Fluoride‐co‐Hexafluoropropylene)−Na3.2Zr1.9Mg0.1Si2PO12 Electrolyte. Energy & Environmental Materials, 6, e12364. https://doi.org/10.1002/eem2.12364
-
Dong, Y., Xu, C., Li, Y., et al. (2023). Ultrahigh‐Rate and Ultralong‐Duration Sodium Storage Enabled by Sodiation‐Driven Reconfiguration. Advanced Energy Materials, 13, 2204324. https://doi.org/10.1002/aenm.202204324
-
Chen, X., Chen, J., Liu, Y., et al. (2023). Advanced Li/Na–CO2 Batteries Enabled by the γ-MnO2 Catalyst with Enhanced Carbonate Decomposition. ACS Applied Materials & Interfaces, 15, 28106–28115. https://doi.org/10.1021/acsami.3c04274
-
Hu, X., Zhang, Y., Wang, P., et al. (2022). Suppression of Gas Crossover and Dendrite Growth in Sodium–Gas Batteries across a Wide Operating Temperature Range. ACS Nano, 16, 17965–17972. https://doi.org/10.1021/acsnano.2c05211
-
Guo, L., Li, B., Thirumal, V., et al. (2019). Advanced rechargeable Na–CO2 batteries enabled by a ruthenium@porous carbon composite cathode with enhanced Na2CO3 reversibility. Chemical Communications, 55, 7946–7949. https://doi.org/10.1039/C9CC02737H
-
Wang, Z., Cai, Y., Ni, Y., et al. (2023). Ultrafine RuO2 nanoparticles/MWCNTs cathodes for rechargeable Na-CO2 batteries with accelerated kinetics of Na2CO3 decomposition. Chinese Chemical Letters, 34, 107405. https://doi.org/10.1016/j.cclet.2022.04.003
-
Lu, Y., Cai, Y., Zhang, Q., et al. (2019). A compatible anode/succinonitrile-based electrolyte interface in all-solid-state Na–CO2 batteries. Chemical Science, 10, 4306–4312. https://doi.org/10.1039/C8SC05178J
-
Ge, B., Lee, H., Im, J., et al. (2023). Engineering an atomic-level crystal lattice and electronic band structure for an extraordinarily high average thermoelectric figure of merit in n-type PbSe. Energy & Environmental Science, 16, 3994–4008. https://doi.org/10.1039/D3EE01226C
-
Ding, Y., Sun, X., Lin Wang, Z., et al. (2012). Misfit dislocations in multimetallic core-shelled nanoparticles. Applied Physics Letters, 100, 111603. https://doi.org/10.1063/1.3695332
-
Francis, M. F., Neurock, M. N., Zhou, X. W., et al. (2008). Atomic assembly of Cu/Ta multilayers: Surface roughness, grain structure, misfit dislocations, and amorphization. Journal of Applied Physics, 104, 034310. https://doi.org/10.1063/1.2968240
-
Niu, W., Chen, Z., Guo, W., et al. (2023). Pb-rich Cu grain boundary sites for selective CO-to-n-propanol electroconversion. Nature Communications, 14, 4882. https://doi.org/10.1038/s41467-023-40689-w
-
Zhang, Q., Chu, Y., Wu, J., et al. (2024). Mitigating Planar Gliding in Single‐Crystal Nickel‐Rich Cathodes through Multifunctional Composite Surface Engineering. Advanced Energy Materials, 14, 2303764. https://doi.org/10.1002/aenm.202303764
-
Zhang, Q., Wang, Y., Deng, Q., et al. (2024). In situ and Real‐time Monitoring the Chemical and Thermal Evolution of Lithium‐ion Batteries with Single‐crystalline Ni‐rich Layered Oxide Cathode. Angewandte Chemie, 136, e202401716. https://doi.org/10.1002/ange.202401716
-
Hammer, B., Nørskov, J. (1995). Electronic factors determining the reactivity of metal surfaces. Surface Science, 343, 211–220. https://doi.org/10.1016/0039-6028(96)80007-0
-
Linck, M., Hartel, P., Uhlemann, S., et al. (2016). Chromatic Aberration Correction for Atomic Resolution TEM Imaging from 20 to 80 kV. Physical Review Letters, 117, 076101. https://doi.org/10.1103/PhysRevLett.117.076101
-
Li, Z., Qin, H., Tian, W., et al. (2024). 3D Sb‐Based Composite Framework with Gradient Sodiophilicity for Ultrastable Sodium Metal Anodes. Advanced Functional Materials, 34, 2301554. https://doi.org/10.1002/adfm.202301554
-
Liu, Y., Bai, M., Du, D., et al. (2023). Affinity‐Engineered Flexible Scaffold toward Energy‐Dense, Highly Reversible Na Metal Batteries. Energy & Environmental Materials, 6, e12350. https://doi.org/10.1002/eem2.12350
-
Bao, C., Wang, J., Wang, B., et al. (2022). 3D Sodiophilic Ti3C2 MXene@g-C3N4 Hetero-Interphase Raises the Stability of Sodium Metal Anodes. ACS Nano, 16, 17197–17209. https://doi.org/10.1021/acsnano.2c07771
-
Li, Z., Zhang, Y., Guan, H., et al. (2023). Rationally Integrating 2D Confinement and High Sodiophilicity toward SnO2/Ti3C2Tx Composites for High‐Performance Sodium‐Metal Anodes. Small, 19, 2208277. https://doi.org/10.1002/smll.202208277
-
Xie, Y., Hu, J., Han, Z., et al. (2020). Encapsulating sodium deposition into carbon rhombic dodecahedron guided by sodiophilic sites for dendrite-free Na metal batteries. Energy Storage Materials, 30, 1–8. https://doi.org/10.1016/j.ensm.2020.05.008
-
Xiao, H., Li, Y., Chen, W., et al. (2023). Stabilize Sodium Metal Anode by Integrated Patterning of Laser‐Induced Graphene with Regulated Na Deposition Behavior. Small, 19, 2303959. https://doi.org/10.1002/smll.202303959
-
Hou, Z., Wang, W., Yu, Y., et al. (2020). Poly(vinylidene difluoride) coating on Cu current collector for high-performance Na metal anode. Energy Storage Materials, 24, 588–593. https://doi.org/10.1016/j.ensm.2019.06.026
-
Zhuang, R., Zhang, X., Qu, C., et al. (2023). Fluorinated porous frameworks enable robust anode-less sodium metal batteries. Science Advances, 9, eadh8060. https://doi.org/10.1126/sciadv.adh8060
-
Liu, P., Wang, X., Jia, X., et al. (2022). Carbon-Confined Two-Dimensional Sodiophilic Sites Boosted Dendrite-Free Sodium Metal Anodes. ACS Applied Materials & Interfaces, 14, 35873–35882. https://doi.org/10.1021/acsami.2c10929
-
Yuan, R., Liu, P., Wang, X., et al. (2023). Interlayer Sodium Plating/Stripping in Van der Waals‐Layered Quantum Dot Superstructure. Small, 19, 2300919. https://doi.org/10.1002/smll.202300919
-
Xiao, J., Xiao, N., Li, K., et al. (2022). Sodium Metal Anodes with Self‐Correction Function Based on Fluorine‐Superdoped CNTs/Cellulose Nanofibrils Composite Paper. Advanced Functional Materials, 32, 2111133. https://doi.org/10.1002/adfm.202111133
-
Yue, L., Qi, Y., Niu, Y., et al. (2021). Low‐Barrier, Dendrite‐Free, and Stable Na Plating/Stripping Enabled by Gradient Sodiophilic Carbon Skeleton. Advanced Energy Materials, 11, 2102497. https://doi.org/10.1002/aenm.202102497
-
Zhang, Q., Lu, Y., Zhou, M., et al. (2018). Achieving a stable Na metal anode with a 3D carbon fibre scaffold. Inorganic Chemistry Frontiers, 5, 864–869. https://doi.org/10.1039/C7QI00802C
-
Xu, M., Liu, Z., Li, Y., et al. (2023). Uniform SnSe nanoparticles on 3D graphene host enabling a dual-nucleation-site interface for dendrite-free sodium metal batteries. Energy Storage Materials, 60, 102848. https://doi.org/10.1016/j.ensm.2023.102848
-
Xu, Z., Guo, Z., Madhu, R., et al. (2021). Homogenous metallic deposition regulated by defect-rich skeletons for sodium metal batteries. Energy & Environmental Science, 14, 6381–6393. https://doi.org/10.1039/D1EE01346G
-
Xu, C., Qiu, J., Dong, Y., et al. (2024). Dual‐Functional Electrode Promoting Dendrite‐Free and CO2 Utilization Enabled High‐Reversible Symmetric Na‐CO2 Batteries. Energy & Environmental Materials, 7, e12626. https://doi.org/10.1002/eem2.12626
-
Yang, C., Zhang, Y., Hua, Y., et al. (2023). Functionalized Halloysite Scaffold Controls Sodium Dendrite Growth. ACS Applied Materials & Interfaces, 15, 11949–11960. https://doi.org/10.1021/acsami.3c00261
-
Yang, W., Yang, W., Dong, L., et al. (2021). Hierarchical ZnO nanorod arrays grown on copper foam as an advanced three-dimensional skeleton for dendrite-free sodium metal anodes. Nano Energy, 80, 105563. https://doi.org/10.1016/j.nanoen.2020.105563
-
Li, Y., Wu, F., Li, Y., et al. (2022). Ether-based electrolytes for sodium ion batteries. Chemical Society Reviews, 51, 4484–4536. https://doi.org/10.1039/D1CS00948F
-
Wang, H., Matios, E., Luo, J., et al. (2020). Combining theories and experiments to understand the sodium nucleation behavior towards safe sodium metal batteries. Chemical Society Reviews, 49, 3783–3805. https://doi.org/10.1039/D0CS00033G
-
Adams, B. D., Zheng, J., Ren, X., et al. (2018). Accurate Determination of Coulombic Efficiency for Lithium Metal Anodes and Lithium Metal Batteries. Advanced Energy Materials, 8, 1702097. https://doi.org/10.1002/aenm.201702097
-
Xu, C., Zhan, J., Wang, H., et al. (2021). Dense binary Fe–Cu sites promoting CO2 utilization enable highly reversible hybrid Na–CO2 batteries. Journal of Materials Chemistry A, 9, 22114–22128. https://doi.org/10.1039/D1TA06611K
-
Xu, C., Zhan, J., Wang, Z., et al. (2021). Biomass-derived highly dispersed Co/Co9S8 nanoparticles encapsulated in S, N-co-doped hierarchically porous carbon as an efficient catalyst for hybrid Na–CO2 batteries. Materials Today Energy, 19, 100594. https://doi.org/10.1016/j.mtener.2020.100594
-
Xu, C., Wang, H., Zhan, J., et al. (2022). Engineering NH3-induced 1D self-assembly architecture with conductive polymer for advanced hybrid Na-CO2 batteries via morphology modulation. Journal of Power Sources, 520, 230909. https://doi.org/10.1016/j.jpowsour.2021.230909
-
Huang, W., Qiu, J., Ji, Y., et al. (2023). Exploiting Cation Intercalating Chemistry to Catalyze Conversion-Type Reactions in Batteries. ACS Nano, 17, 5570–5578. https://doi.org/10.1021/acsnano.2c11029
-
Tong, Z., Wang, S., Fang, M., et al. (2021). Na–CO2 battery with NASICON-structured solid-state electrolyte. Nano Energy, 85, 105972. https://doi.org/10.1016/j.nanoen.2021.105972
-
Hu, X., Joo, P. H., Matios, E., et al. (2020). Designing an All-Solid-State Sodium-Carbon Dioxide Battery Enabled by Nitrogen-Doped Nanocarbon. Nano Letters, 20, 3620–3626. https://doi.org/10.1021/acs.nanolett.0c00564
-
Thoka, S., Tong, Z., Jena, A., et al. (2020). High-performance Na–CO2 batteries with ZnCo2O4@CNT as the cathode catalyst. Journal of Materials Chemistry A, 8, 23974–23982. https://doi.org/10.1039/D0TA09235E
-
Wang, X., Zhang, X., Lu, Y., et al. (2018). Flexible and Tailorable Na−CO2 Batteries Based on an All‐Solid‐State Polymer Electrolyte. ChemElectroChem, 5, 3628–3632. https://doi.org/10.1002/celc.201801018
-
Xu, B., Zhang, D., Chang, S., et al. (2022). Fabrication of long-life quasi-solid-state Na-CO2 battery by formation of Na2C2O4 discharge product. Cell Reports Physical Science, 3, 100973. https://doi.org/10.1016/j.xcrp.2022.100973
-
Guan, A., Chen, Z., Quan, Y., et al. (2020). Boosting CO2 Electroreduction to CH4 via Tuning Neighboring Single-Copper Sites. ACS Energy Letters, 5, 1044–1053. https://doi.org/10.1021/acsenergylett.0c00018
-
Tan, C., Wang, A., Cao, D., et al. (2023). Unravelling the Complex Na2CO3 Electrochemical Process in Rechargeable Na‐CO2 Batteries. Advanced Energy Materials, 13, 2204191. https://doi.org/10.1002/aenm.202204191
-
Xu, C., Zhang, K., Zhang, D., et al. (2020). Reversible hybrid sodium-CO2 batteries with low charging voltage and long-life. Nano Energy, 68, 104318. https://doi.org/10.1016/j.nanoen.2019.104318