Defects in Silica and Graphene

December 16, 2013 – Bilayer silica and graphene could hardly be more different in their bonding, yet both form hexagonal 2D lattices. Combining 80 kV aberration-corrected HRTEM with DFT and classical force field calculations, a team from Aalto, Ulm, Helsinki, Vienna, EPFL in Lausanne and the MPI in Stuttgart, with the SALVE project, finds the same defects in both: Stone–Wales and flower defects, reconstructed double vacancies and grain boundaries near 30°. Defects with bond rotations cost less in silica, and at 80 kV only oxygen is knocked out. A 60 kV STEM study from Vienna confirms the double vacancies and their bond rotations in graphene.

Through a combination of aberration-corrected high-resolution transmission electron microscopy (AC-HRTEM) at 80 kV with density functional theory (DFT) and classical force field (CFF) calculations, an international team from Aalto University, Ulm University, the University of Helsinki, the University of Vienna, EPFL in Lausanne and the Max Planck Institute for Solid State Research in Stuttgart, with the participation of the SALVE project, has investigated how the symmetry of a crystal lattice governs its defects and grain boundaries[1]. Such deviations from the ideal lattice determine to a large extent the properties of a material. The team compared two two-dimensional (2D) materials with hexagonal symmetry but very different bonding: hexagonal bilayer silica (HBS) and graphene. Both host the same point defects, Stone–Wales defects, flower defects and reconstructed double vacancies, and both prefer grain boundaries at about 30°. A study published five months later with a Nion UltraSTEM at 60 kV in Vienna serves as validation: it shows the same three double vacancies in graphene turning into one another by bond rotations under the beam.

Two hexagonal 2D materials
For years the family of 2D materials has been growing steadily. One of its members is 2D silica: both a single layer of tetrahedra covalently bonded to the metal substrate and a fully saturated bilayer that is only weakly bound to the substrate have been synthesized[2]–[4]. HBS has great technological potential, for instance as the thinnest oxide gate dielectric, as a support in catalysis[5] or for the isolation of 2D materials from the substrate. Experimentally, 2D silica has been examined with every degree of disorder, from isolated point defects and grain boundaries to a completely amorphous structure[5].

Scientists of the SALVE project took part this year in a study in which the atomic rearrangements in amorphous SiO2 were observed directly for the first time[6]. After numerous studies with scanning tunnelling and atomic force microscopy, which see only the surface, the synthesis of amorphous 2D silica on graphene[7] made it possible to image its atomic structure with low-voltage HRTEM. Now the scientists have published a study on the crystalline phase of 2D silica. “HBS and graphene are by far the most studied hexagonal 2D systems,” said Ute Kaiser, who conducted the experimental imaging by HRTEM. “They have very different binding properties. We wanted to analyze whether the common lattice structure results in similarities concerning the nature of defects.” In HBS, four oxygen atoms form a tetrahedron around each silicon atom, and the tetrahedra share corners in two mirror-image layers (Fig. 1). Leaving out the oxygen atoms, the silicon atoms form the same hexagonal network as the carbon atoms of graphene.

What the electron beam can knock out
As they had done before for graphene[8] and transition metal dichalcogenides[9], the scientists calculated the displacement threshold Td of oxygen and silicon atoms in HBS with DFT-based molecular dynamics. Td is the minimum kinetic energy an atom needs to leave the lattice. It came out at 16.8 eV for Si and 11.6 eV for O. At the 80 keV electron energy used for imaging, only oxygen atoms are therefore ejected, while the energy transferred to Si atoms stays below their threshold (Fig. 2). Many topological transformations of HBS under the electron beam are thus driven by a lack of oxygen in the lattice.

Point defects
The study relates the crystalline and amorphous structures through bond rotations, an idea known for sp2 carbon systems since 1986[10]. Point defects that can be created by one bond rotation are called Stone–Wales (SW) defects after their discoverers[10]. In graphene the rotation turns the bond between two neighbouring C atoms by 90°; in HBS it turns four Si atoms, two in each layer, together with the neighbouring O atoms (Fig. 3). The AC-HRTEM images at 80 kV show the SW defect in both materials, as well as a flower defect[11], which forms by six successive bond rotations and is essentially a small grain turned by 30° against the surrounding lattice. Both defects keep the atomic density of the pristine lattice. They also show a double vacancy of the 5555-6-7777 type, the so-called butterfly defect[12], created by removing two neighbouring structural units and performing two bond rotations, and a defect with two added units. All of them occur in both materials; the images are shown side by side with those of a later STEM study in the validation box below.

The calculated formation energies differ most for defects that involve rotations: these are lower in HBS. The simple 5-8-5 double vacancy costs about 9 eV in HBS but only about 7.5 eV in graphene; after one rotation (555-777) the order is reversed, and after a second one (5555-6-7777) even more clearly. The flower defect costs only 1.2 eV in HBS, but 7.0 eV in graphene. The numbers are compared in the box below, which also holds the models of the double vacancies (Fig. 4).

▸ Comparison: bilayer silica vs. graphene

To understand why rotations are cheaper in HBS, the team calculated the energy of every step from the crystal to the flower defect (Fig. 5). As in graphene, the energy first rises with each rotation and falls again from the fourth rotation on, until the flower defect is reached. The strain field around the flower defect reaches much less far than those of the intermediate defects: as in graphene, the energy is lowest when the defect is turned by 30° against the surrounding lattice, because its 5-7 pairs are packed so closely that their elastic fields cancel. Unlike graphene, HBS allows additional relaxation in the dislocation cores, because its tetrahedral building blocks can rotate.

Bond rotations under the beam
In graphene a bond rotation involves only two atoms, yet its energy barrier is so high that heat alone can never drive it; an electron impact during imaging can. For the far more complex HBS, such a transformation might seem impossible. Nevertheless, successive AC-HRTEM images clearly show it, both the annihilation of an SW defect in disordered HBS and the appearance of SW defects in crystalline areas (Fig. 6). The details stay hidden, but the transformation is certainly a sequence of several steps in which the atoms shift gradually from the 5-7 to the 6-6 geometry, not the rigid rotation of a dimer sketched in Fig. 3. The calculations suggest how the beam can drive it: removing the two oxygen atoms that bridge the central pair lowers the formation energy of the SW defect by about 0.5 eV, so oxygen vacancies, created by the beam and refilled by atoms from the surroundings, lower the barrier for rotations.

Extended topological defects
Crystalline HBS frequently consists of small grains, most of them turned by about 30° against each other (Fig. 7a). As earlier for graphene[13], one-dimensional defects served as idealized models of grain boundaries, ignoring their curved shapes. Only boundaries analogous to those in graphene were studied; direct Si–Si bonds, similar to the Mo–Mo and S–S bonds recently observed in MoS2[14], were not taken into account. The geometry of a (1,0) grain boundary is shown in Fig. 7b. Compared with graphene[13], the calculated formation energies vary markedly less smoothly with the angle (Fig. 7c), presumably because the tetrahedra can rotate and so relax the structure further.

To find the preferred orientation of the boundaries, the DFT and CFF values were fitted with the analytic Read–Shockley expression[15]. The ratio of the Burgers vector to the core radius, which decides how fast the energy falls at large angles, is about 1 for HBS but about 2 for graphene[13], so the energies at large angles are much lower in HBS. All boundary types studied tend to low formation energies near 30°, in agreement with the experimental observations for graphene[13] as well as for HBS.

Haeckelite structures
Haeckelites are lattices made of 5- and 7-membered rings instead of hexagons; they were proposed theoretically for graphene[16] but never found experimentally. They represent an extreme case of defect concentration and of strain. Since the HBS samples shrank constantly under the beam, which points to high strain, the team also calculated how strain changes the formation energy of the SW defect, which can even become negative (Fig. 8a). Two Haeckelite structures of HBS cost only 73 and 33 meV per SiO2 unit more than the hexagonal lattice (Fig. 8b, c), much less than in graphene. This may explain why 2D amorphous silica grows on metals, while graphene becomes amorphous only under special irradiation[17]. How well the classical force field reproduces the DFT values is shown in the box below.

▸ Validation: DFT vs. classical force field

Similarities and differences
Although HBS and graphene contain different atoms and have structures of very different complexity, defects behave qualitatively alike in both, the point defects such as SW defects as well as extended defects such as grain boundaries. These two systems thus differ considerably from 2D systems such as the transition metal dichalcogenides[14], which consist of several elements and have trigonal symmetry. In those, the network links are more constrained, and SW transformations are much less likely because they would create bonds between like atoms. Despite experimental effort[19], SW defects have never been observed in h-BN. Since both sp2 carbon and bilayer silica can form amorphous structures and possibly Haeckelites, the study suggests that defect structures will be comparable in any hexagonal 2D system, regardless of the complexity of its structural units. Such systems may include epitaxial atomically thin silicon[20] and epitaxial transition metal networks[21].

The most significant difference lies in how defects form and move. Because many more atoms take part, this is far more complex in HBS. The momentum of an imaging electron is never transferred to a complete structural unit of the silica lattice, but only to a single atom within it. Most astonishing is that the SW transformation is observable in silica at all. As explanation, the scientists propose that the electron beam drives these processes because the vacancies left by sputtered oxygen atoms, and the strain they induce, lower the barriers for displacing atoms.

Validation: FEI Titan at 80 kV vs. Nion UltraSTEM at 60 kV
Five months later, Jani Kotakoski, one of the authors, with Clemens Mangler and Jannik C. Meyer at the University of Vienna, followed one double vacancy in graphene for 13 minutes with a Nion UltraSTEM 100 scanning TEM at 60 kV in ultrahigh vacuum[25]. Double vacancies are the first step on the way from the crystal to an amorphous network, which the Ulm study traces through bond rotations in both materials and which had been followed in graphene at 80 and 100 kV up to a two-dimensional amorphous carbon[17]. The box below compares the two microscopes and shows the defects of both side by side (Fig. 9).

▸ Validation: FEI Titan at 80 kV vs. Nion UltraSTEM at 60 kV

Challenges named by the authors
HRTEM shows the atomic rearrangements directly, but the details of the SW transformation in HBS remain unclear: the time resolution is about one second, the out-of-plane motion of the Si atoms cannot be seen, and the oxygen atoms give only poor contrast[1]. The grain boundaries were modelled as straight lines, while real ones are curved, and boundaries without oxygen and with direct Si–Si bonds were not calculated. The fixed supercells described isolated defects only; at higher defect concentrations, relaxing the cell lowers the energies further. The samples shrank constantly under the beam, so the strain during imaging was high and not controlled. How the 3D shear modulus should be defined for a 2D bilayer is not unambiguous either.

▸ Recipe: samples and calculations

Outlook
“In the future, perhaps far more suspended hexagonal materials can be produced, which can also provide additional opportunities for study of general trends in the defect energetics and morphology,” Kaiser said.

Resource:
Björkman, T., Kurasch, S., Lehtinen, O., Kotakoski, J., Yazyev, O. V., Srivastava, A., Skákalová, V., Smet, J. H., Kaiser, U., Krasheninnikov, A. V. (2013).
Defects in bilayer silica and graphene: common trends in diverse hexagonal two-dimensional systems.
Sci. Rep. 3, 3482.
https://doi.org/10.1038/srep03482

Download this news article as PDF – for reading on paper, taking notes or filing.

References
  1. Björkman, T., Kurasch, S., Lehtinen, O., Kotakoski, J., Yazyev, O. V., Srivastava, A., Skakalova, V., Smet, J. H., Kaiser, U., & Krasheninnikov, A. V. (2013). Defects in Bilayer Silica and Graphene: Common Trends in Diverse Hexagonal Two-Dimensional Systems. Scientific Reports, 3, 3482. https://doi.org/10.1038/srep03482

  2. Weissenrieder, J., Kaya, S., Lu, J.-L., Gao, H.-J., Shaikhutdinov, S., Freund, H.-J., Sierka, M., Todorova, T. K., & Sauer, J. (2005). Atomic Structure of a Thin Silica Film on a Mo(112) Substrate: A Two-Dimensional Network of SiO4 Tetrahedra. Physical Review Letters, 95(7), 076103. https://doi.org/10.1103/PhysRevLett.95.076103

  3. Löffler, D., Uhlrich, J. J., Baron, M., Yang, B., Yu, X., Lichtenstein, L., Heinke, L., Büchner, C., Heyde, M., Shaikhutdinov, S., Freund, H.-J., Włodarczyk, R., Sierka, M., & Sauer, J. (2010). Growth and Structure of Crystalline Silica Sheet on Ru(0001). Physical Review Letters, 105(14), 146104. https://doi.org/10.1103/PhysRevLett.105.146104

  4. Yang, B., Boscoboinik, J. A., Yu, X., Shaikhutdinov, S., & Freund, H.-J. (2013). Patterned Defect Structures Predicted for Graphene Are Observed on Single-Layer Silica Films. Nano Letters, 13(9), 4422–4427. https://doi.org/10.1021/nl402264k

  5. Shaikhutdinov, S., & Freund, H.-J. (2013). Ultrathin Silica Films on Metals: The Long and Winding Road to Understanding the Atomic Structure. Advanced Materials, 25(1), 49–67. https://doi.org/10.1002/adma.201203426

  6. Huang, P. Y., Kurasch, S., Alden, J. S., Shekhawat, A., Alemi, A. A., McEuen, P. L., Sethna, J. P., Kaiser, U., & Muller, D. A. (2013). Imaging Atomic Rearrangements in Two-Dimensional Silica Glass: Watching Silica’s Dance. Science, 342(6155), 224–227. https://doi.org/10.1126/science.1242248

  7. Huang, P. Y., Kurasch, S., Srivastava, A., Skakalova, V., Kotakoski, J., Krasheninnikov, A. V., Hovden, R., Mao, Q., Meyer, J. C., Smet, J., Muller, D. A., & Kaiser, U. (2012). Direct Imaging of a Two-Dimensional Silica Glass on Graphene. Nano Letters, 12(2), 1081–1086. https://doi.org/10.1021/nl204423x

  8. Meyer, J. C., Eder, F., Kurasch, S., Skakalova, V., Kotakoski, J., Park, H. J., Roth, S., Chuvilin, A., Eyhusen, S., Benner, G., Krasheninnikov, A. V., & Kaiser, U. (2012). Accurate Measurement of Electron Beam Induced Displacement Cross Sections for Single-Layer Graphene. Physical Review Letters, 108(19), 196102. https://doi.org/10.1103/PhysRevLett.108.196102

  9. Komsa, H.-P., Kotakoski, J., Kurasch, S., Lehtinen, O., Kaiser, U., & Krasheninnikov, A. V. (2012). Two-Dimensional Transition Metal Dichalcogenides Under Electron Irradiation: Defect Production and Doping. Physical Review Letters, 109(3), 035503. https://doi.org/10.1103/PhysRevLett.109.035503

  10. Stone, A. J., & Wales, D. J. (1986). Theoretical Studies of Icosahedral C60 and Some Related Species. Chemical Physics Letters, 128(5–6), 501–503. https://doi.org/10.1016/0009-2614(86)80661-3

  11. Cockayne, E. (2012). Graphing and Grafting Graphene: Classifying Finite Topological Defects. Physical Review B, 85(12), 125409. https://doi.org/10.1103/PhysRevB.85.125409

  12. Zubeltzu, J., Chuvilin, A., Corsetti, F., Zurutuza, A., & Artacho, E. (2013). Knock-on Damage in Bilayer Graphene: Indications for a Catalytic Pathway. Physical Review B, 88(24), 245407. https://doi.org/10.1103/PhysRevB.88.245407

  13. Yazyev, O. V., & Louie, S. G. (2010). Topological Defects in Graphene: Dislocations and Grain Boundaries. Physical Review B, 81(19), 195420. https://doi.org/10.1103/PhysRevB.81.195420

  14. Najmaei, S., Liu, Z., Zhou, W., Zou, X., Shi, G., Lei, S., Yakobson, B. I., Idrobo, J.-C., Ajayan, P. M., & Lou, J. (2013). Vapour Phase Growth and Grain Boundary Structure of Molybdenum Disulphide Atomic Layers. Nature Materials, 12(8), 754–759. https://doi.org/10.1038/nmat3673

  15. Read, W. T., & Shockley, W. (1950). Dislocation Models of Crystal Grain Boundaries. Physical Review, 78(3), 275–289. https://doi.org/10.1103/PhysRev.78.275

  16. Appelhans, D. J., Lin, Z., & Lusk, M. T. (2010). Two-Dimensional Carbon Semiconductor: Density Functional Theory Calculations. Physical Review B, 82(7), 073410. https://doi.org/10.1103/PhysRevB.82.073410

  17. SALVE news (2011). From Graphene to 2D Amorphous Carbon. salve-project.de, March 9, 2011. https://salve-project.de/newspress/from-graphene-to-two-dimensional-amorphous-carbon.html

  18. Watanabe, T., Fujiwara, H., Noguchi, H., Hoshino, T., & Ohdomari, I. (1999). Novel Interatomic Potential Energy Function for Si, O Mixed Systems. Japanese Journal of Applied Physics, 38(4A), L366–L369. https://doi.org/10.1143/JJAP.38.L366

  19. Alem, N., Erni, R., Kisielowski, C., Rossell, M. D., Gannett, W., & Zettl, A. (2009). Atomically Thin Hexagonal Boron Nitride Probed by Ultrahigh-Resolution Transmission Electron Microscopy. Physical Review B, 80(15), 155425. https://doi.org/10.1103/PhysRevB.80.155425

  20. Vogt, P., De Padova, P., Quaresima, C., Avila, J., Frantzeskakis, E., Asensio, M. C., Resta, A., Ealet, B., & Le Lay, G. (2012). Silicene: Compelling Experimental Evidence for Graphenelike Two-Dimensional Silicon. Physical Review Letters, 108(15), 155501. https://doi.org/10.1103/PhysRevLett.108.155501

  21. Li, L., Wang, Y., Xie, S., Li, X.-B., Wang, Y.-Q., Wu, R., Sun, H., Zhang, S., & Gao, H.-J. (2013). Two-Dimensional Transition Metal Honeycomb Realized: Hf on Ir(111). Nano Letters, 13(10), 4671–4674. https://doi.org/10.1021/nl4019287

  22. Blöchl, P. E. (1994). Projector Augmented-Wave Method. Physical Review B, 50(24), 17953–17979. https://doi.org/10.1103/PhysRevB.50.17953

  23. Kresse, G., & Furthmüller, J. (1996). Efficiency of Ab-Initio Total Energy Calculations for Metals and Semiconductors Using a Plane-Wave Basis Set. Computational Materials Science, 6(1), 15–50. https://doi.org/10.1016/0927-0256(96)00008-0

  24. Nordlund, K. (1995). Molecular Dynamics Simulation of Ion Ranges in the 1–100 keV Energy Range. Computational Materials Science, 3(4), 448–456. https://doi.org/10.1016/0927-0256(94)00085-Q

  25. Kotakoski, J., Mangler, C., & Meyer, J. C. (2014). Imaging Atomic-Level Random Walk of a Point Defect in Graphene. Nature Communications, 5, 3991. https://doi.org/10.1038/ncomms4991