April 1, 2011 – Slow electrons spare the sample, but for decades they gave blurred images. Researchers from Ulm University, CEOS in Heidelberg, Carl Zeiss in Oberkochen, Vienna and Nottingham characterized the prototype SALVE microscope, a monochromated Zeiss Libra 200 with a CEOS aberration corrector, at only 20 kV. It resolves lattice fringes of 272 pm in silicon and 213 pm in single-layer graphene, C60 fullerenes in a nanotube withstand about a hundred times the dose that destroys them at 80 kV, and EELS at 20 kV measures band gaps and refractive indices of Si and Ge. Studies from Berkeley, Harvard, Nion and AIST at 20 to 80 kV confirm it: low voltage protects the sample, and chromatic aberration sets the limit.

Lowering the voltage of an electron microscope protects delicate samples, but it also blurs the image. A team from Ulm University, CEOS in Heidelberg, Carl Zeiss in Oberkochen, the Vienna University of Technology and the University of Nottingham, led by Ute Kaiser, has now characterized the prototype of the SALVE microscope at an accelerating voltage of only 20 kV[1]. The instrument, a Zeiss Libra 200 with an electrostatic monochromator and a CEOS Cs corrector, resolves lattice fringes of 272 pm in 4 nm thin silicon and of 213 pm in single-layer graphene. C60 fullerenes inside a carbon nanotube withstand about a hundred times the electron dose that destroys them at 80 kV, and electron energy-loss spectroscopy (EELS) at 20 kV measures band gaps and refractive indices of silicon and germanium. Four studies from Berkeley, Harvard, Nion and AIST, made with other microscopes between 20 and 80 kV, serve as validation: low voltage protects the sample, and the chromatic aberration sets the limit.

Why go down to 20 kV
Aberration-corrected transmission electron microscopy (TEM) images materials atom by atom with electrons of medium energy[2],[3]. Often, however, the sample and not the instrument limits the resolution, because the beam damages it[4],[5]. Ionization and heating depend on the beam current, but knock-on damage, in which an electron kicks an atom out of its place, depends only on the electron energy. It can be avoided only by working below the knock-on threshold of the material under study. More than 45 years ago, a 6 kV instrument already imaged biological samples with high contrast, but its large chromatic aberration ruined the resolution[6], and low voltages in TEM were abandoned for decades. Aberration correctors brought them back[5]: a doubly corrected low-voltage TEM for 30 to 60 kV was being designed at AIST in Tsukuba[7], and the Nion UltraSTEM had reached atomic resolution at 60 kV in scanning mode[8].

The SALVE (Sub-Ångström Low-Voltage Electron microscopy) project aimed further: a new corrector for both chromatic and spherical aberration (Cc/Cs) for electron energies down to 20 keV. The idea rests on a simple balance. The dose a sample can tolerate times the contrast it gives is nearly independent of the voltage, and the contrast rises as the voltage falls. As long as the instrumental resolution does not get worse, a lower voltage therefore gives a sharper image of a radiation-sensitive object[5]. The samples must then be very thin, much thinner than 10 nm at 20 kV. For single molecules, the team planned graphene as the thinnest possible conducting support[9], whose lattice can be removed from the image by Fourier filtering[10]. For spectroscopy, low voltage has a further advantage: relativistic energy losses such as Cerenkov radiation, which mask the band gap in EELS, are reduced or avoided[11],[12]. For silicon their limit lies between 15 and 20 kV, for germanium below 5 kV[12].

The prototype at 20 kV
The prototype SALVE microscope was a monochromated Zeiss Libra 200 MC with an in-column corrected OMEGA energy filter and a hexapole Cs corrector from CEOS. At 20 kV the monochromator narrowed the energy spread of the beam to 0.17 or 0.15 eV, depending on the slit, and the energy filter was always on. The authors first measured how far the instrument transfers information. The chromatic aberration coefficient Cc came out at 1.2 ± 0.1 mm, in good agreement with the calculated 1.26 mm. Without the monochromator, at an energy spread of 0.75 eV, chromatic aberration limits the resolution to about 0.52 nm. With the monochromator at 0.17 eV, the limit moves to 0.25 nm. Diffractograms with Young’s fringes confirm this: at 20 kV the fringes reached 440 pm without and 240 pm with the monochromator. At 80 kV the same microscope transferred information to 85 pm with the monochromator, while a Zeiss Libra at Harvard reached 117 pm at 80 kV without it (Fig. 1)[13]. With the illumination tilted by 30 mrad, the image spread, which collects all lateral instabilities, turned out to be better than 0.18 nm[14].

Up to fifth order, the hexapole corrector leaves two intrinsic aberrations: the six-fold astigmatism A5 = 15 mm and the fifth-order spherical aberration C5 = 21 mm. The six-fold astigmatism reaches the usual tolerance of a quarter wavelength (π/4) at a scattering angle of 27 mrad, which corresponds to 0.31 nm at 20 kV. The measured aberrations allowed a well-corrected state up to this angle. In a microscope with a monochromator, the hexapole corrector thus serves for phase-contrast imaging at 20 kV up to the limit set by its own six-fold astigmatism. The planned Cc/Cs corrector of the final SALVE instrument was designed to push this limit to 50 mrad, or 0.17 nm at 20 kV[1].

Silicon and graphene
A 4 nm thin silicon lamella, viewed along [110], served as the crystalline test (Fig. 2). With the monochromator, the 111 fringes (314 pm) and the 200 fringes (272 pm) are clearly visible in the image. Without it, they show only weakly in the Fourier transform. The authors attributed the 222 reflections (157 pm), which also appeared, to dynamical diffraction. Such line resolution at 20 kV demonstrated the mechanical and electrical stability of the system.

Single-layer graphene is a much harder test, because it scatters weakly and its 213 pm lattice spacing corresponds to about 40 mrad at 20 kV, beyond the reach of axial illumination. The team therefore tilted the beam by 30 mrad, which the Cs corrector allows without coma or field astigmatism[14]. With tilt and defocus adjusted, all six first-order reflections of graphene appeared in a single unfiltered exposure. Optimized for one lattice direction, the lattice modulated the image by 2.5 % of the mean intensity. Electrons scattered to 40 mrad thus still contributed to the contrast. The comparison with 80 kV shows what the lower voltage costs (Fig. 3): at 80 kV the same microscope images the honeycomb lattice directly, at 20 kV the lattice is barely visible in the raw image, the Fourier transform reveals the 213 pm reflections, and only Bragg filtering brings the honeycomb out in the image (Fig. 3c).

Fullerenes last a hundred times longer
The real reason for going to 20 kV is the sample. The team filled double-walled carbon nanotubes with C60 fullerenes and recorded dose series at 80 and 20 kV (Fig. 4). Fullerenes, built from pentagons and hexagons, have much weaker bonds than nanotubes, which consist only of hexagons; defect-free nanotubes stay intact at 80 kV and below[15]. At 80 kV the fullerenes began to coalesce and polymerize after about 107 electrons per nm2. After 109 electrons per nm2, almost all of them were damaged and had started to fuse into a third tube inside the double-walled one. At 20 kV, the same dose caused only very few changes. The beam damage was thus reduced by a factor of about 100, and the images at 20 kV showed, as theory predicts, much higher contrast. The atomic lattice of molecules and tubes was not yet resolved: at such low voltage, chromatic aberration limits the resolution, a limit the Cc/Cs corrector of the final SALVE instrument was built to remove[1].

Spectroscopy at 20 kV
In spectroscopy mode, the monochromated 20 keV beam gives spectra with exceptionally low background (Fig. 5). For 10 nm thick silicon, the zero-loss peak was 0.11 eV wide at half maximum and 1.0 eV at one thousandth of its maximum, which matters for an accurate band gap. Spectral details between about 2.6 and 7 eV that are otherwise smeared out became visible, followed by the surface plasmon at 9 eV and the volume plasmon at 16.7 eV. EELS covers a much wider energy range than optical methods. After removing the zero-loss peak and plural scattering, the authors found a direct band gap of 2.6 eV for silicon, in very good agreement with band-structure calculations[16]. For germanium, a direct band gap of 0.80 ± 0.03 eV followed after residual relativistic losses had been removed with an iterative routine[17]. For the first time, a TEM thus determined band gaps and refractive indices of Si and Ge as functions of the energy loss. How these values compare with optical data and calculations is shown in the box below, which also holds the refractive indices (Figs. 6 and 7).

▸ Validation: measurement vs. calculation and optical data

Other microscopes, same conclusion
Around the same time, groups with other microscopes worked between 20 and 80 kV. The Berkeley and Harvard studies appeared in 2012 but were finished in 2011, one submitted in November, the other online in December, so all of them show where the effort to overcome the challenge of chromatic aberrations at low primary energies stood in 2011. At Lawrence Berkeley National Laboratory, the TEAM 0.5 imaged silicon at 80, 50 and 20 kV; at Harvard, a Zeiss Libra 200 of the same family as the SALVE prototype reached atomic resolution at 80 and 40 kV; Nion and Oak Ridge National Laboratory imaged nanotubes, fullerenes and graphene with the UltraSTEM at 60 kV; and AIST in Tsukuba compared fullerenes at 30 and 60 kV in a JEOL 2100F STEM. Each of them is compared with the Ulm prototype in its own box. The first box holds the Berkeley images of silicon (Figs. 8 and 9).

▸ Validation: Zeiss Libra 200 at 20 kV vs. FEI TEAM 0.5 at 20–80 kV

Harvard used a microscope of the same family as the SALVE prototype and went down to 40 kV; the box below holds its nanotube, graphene and silicon images (Figs. 10, 11 and 12).

▸ Validation: Zeiss Libra 200 at 80 kV vs. Zeiss Libra 200 at 80 and 40 kV

In scanning mode, the Nion UltraSTEM imaged fullerenes in nanotubes, graphene and a nanotube wall at 60 keV (Figs. 13, 14 and 15).

▸ Validation: Zeiss Libra 200 at 80 kV vs. Nion UltraSTEM at 60 and 40 keV

At AIST, the same kind of fullerene-filled nanotube was compared at 30 and 60 kV (Fig. 16).

▸ Validation: Zeiss Libra 200 at 20 kV vs. JEOL 2100F at 30 and 60 kV

Put side by side, the resolution reached by all five microscopes follows the chromatic limit (Fig. 17). The three Cs-corrected TEMs measured Young’s fringes at 20 and 40 kV and lie just above the curve calculated for a Cc of 1.2 mm and an energy spread of 100 meV[20]; the JEOL scanning microscope, with 111 pm at 30 kV and 96 pm at 60 kV, lies in the same range[24]. The Nion UltraSTEM, with about 110 pm at 60 keV and 123 pm at 40 keV, compares with the TEMs at about 20 kV higher voltage, not with those at 20 kV[8],[22]. At 80 kV the same three TEMs reach 85 to 95 pm[13],[19]; there the chromatic limit is no longer the bottleneck, and the fixed fifth-order spherical aberration takes over[20]. Across the SALVE range from 20 to 80 kV, the resolution of a Cs-corrected instrument thus falls from below 100 pm to about 200 pm, and without Cc correction 20 kV stays at about 200 pm, whatever the brand of the instrument.

Challenges named by the authors
At 20 kV, chromatic aberration still limited the resolution: the lattices of the fullerenes and nanotubes were not resolved, and smaller monochromator slits did not help, because they cost too much intensity[1]. The hexapole corrector itself limits phase contrast to 27 mrad through its six-fold astigmatism. The CCD camera converted each 20 keV electron into only 0.5 counts, compared with at least 5 counts at medium voltage, so many more electrons were needed to rise above the readout noise. Samples must be much thinner than 10 nm, while conventional focused-ion-beam lift-out gives 20–30 nm at best, and they must be homogeneous and free of surface contamination. Because the spectrometer disperses so strongly at 20 kV, only a small part of the spectrum fits on the camera, and the cut-off spectrum needs matrix instead of Fourier deconvolution. Thin samples also enhance surface plasmons, and the missing 4.5 eV feature of silicon and the transition strengths of germanium remained unexplained.

▸ Recipe: samples and measurements

A low-voltage tool for sensitive matter
The study showed that a carefully stabilized, monochromated and Cs-corrected TEM gives lattice resolution, high contrast and gentle imaging at 20 kV, and that EELS at this voltage opens the band-gap region to measurement in nearly all materials. “These very first results demonstrate that low kV TEM is an exciting new tool for determination of structural and electronic properties of different types of nano-materials,” the authors write[1]. The final SALVE instrument, with a Cc/Cs corrector and an optimized detector, was meant to bring atomic resolution to imaging and spectroscopy of radiation-sensitive objects. The work was supported by the German Research Foundation (DFG) and the Ministry of Science, Research and the Arts of Baden-Württemberg within the SALVE project.

Resource:
Kaiser, U., Biskupek, J., Meyer, J. C., Leschner, J., Lechner, L., Rose, H., Stöger-Pollach, M., Khlobystov, A. N., Hartel, P., Müller, H., Haider, M., Eyhusen, S., & Benner, G. (2011).
Transmission electron microscopy at 20 kV for imaging and spectroscopy.
Ultramicroscopy 111(8), 1239–1246.
https://doi.org/10.1016/j.ultramic.2011.03.012

Update – April 29, 2014

The news article of April 1, 2011 ends above. Later work is listed below.

Down to 15 kV in Tsukuba
A Cs-corrected STEM at 15 keV compares with a Cs-corrected TEM at 20 kV. The JEOL and AIST team took its low-voltage microscope with cold field emission gun and delta corrector down to 15 kV[27]. In a raw ADF STEM image, silicon [110] showed the {111}, {002} and {220} planes of 314, 272 and 192 pm, and its power spectrum reached 164 pm (Fig. 18); in TEM, the {200} and {220} fringes of 272 and 192 pm appeared, with spots in the power spectrum out to 111 pm. The silicon {111} and {200} fringes at 314 and 272 pm are the same ones the SALVE prototype resolved at 20 kV; side by side at the same scale, both images show the silicon lattice (Fig. 18c).

Update – September 1, 2014

Dose rate instead of voltage? A claim from LBNL and co-workers
LBNL and co-workers imaged graphene and catalytic nanoparticles on the TEAM 0.5 at 80 kV with very low dose rates[28]. Below a critical dose rate of about 104 electrons per nm2 and second, the structures stayed intact. From this they concluded that lowering the beam current matters more than lowering the voltage: “changing the wavelength of the incoming electrons without reducing the number of them reaching the sample per unit time has a lower influence on the beam–sample mechanisms of interaction.” For graphene it went further: below 20 kV, radiolysis sets in and material is removed from the sample “also at a rapid rate”.

LBNL and co-workers, TEAM 0.5 [28]Ulm, SALVE I and SALVE IIIAgreement
Set-up
Voltages studied80 kV only20, 30, 60 and 80 kV–
Results
Voltage vs. dose ratelowering the voltage has “a lower influence” than lowering the dose rateC60: about 100 times more dose at 20 than at 80 kV (Fig. 4) [1]; graphene edge fixed at 30 kV, unstable at 80 kV [29]refuted for Ulm
Graphene at low voltageradiolysis below 20 kV removes material “at a rapid rate” (unpublished)at 20 kV a hole grows by about one unit cell per edge per 108 e/nm2 [30]; conductivity largely suppresses radiolysis [31]refuted for graphene at 20 kV
Dose ratebelow about 104 e/(nm2 s) at 80 kV graphene and nanoparticles stay intactcarbon monolayers at the same moderate dose rate: holes grow at 80 kV, almost not at 60 kV [31]yes for dose rate; voltage counts as well
40 kV“proved to be successful” for graphene (cited)part of the SALVE range of 20–80 kVyes (their own admission)

Table 6: Claims of LBNL and co-workers and the Ulm results.

The paper itself did not test the voltage. All its measurements were made at one energy, as the authors write: “results shown in this investigation for 80 keV”. The graphene claim rests on “Calderon, unpublished research”, and it concerns energies below 20 kV, the lower end of the SALVE range. The paper also concedes that a lower voltage helped: “Using a slightly higher energy (40 keV) has proved to be successful … for the observation of graphene and other nanomaterials”[28]. The Ulm results refute the general claim point by point (Table 6). At the same dose, C60 fullerenes lasted about a hundred times longer at 20 kV than at 80 kV (Fig. 4). With the SALVE III microscope, an edge configuration in graphene stays fixed at 30 kV, whereas it is reproducibly unstable at 80 kV[29]. At 20 kV, a hole in graphene grew by only about one unit cell per edge per 108 electrons per nm2 (3D Imaging of Graphene)[30]. In nanocrystalline carbon monolayers at the same moderate dose rate, the hole growth that dominated at 80 kV almost stopped at 60 kV (Grain Boundary Engineering)[31]. Dose rate and voltage are not alternatives: knock-on damage depends only on the electron energy, ionization and heating on the beam current, and the high electrical conductivity of graphene largely suppresses radiolysis[31]. SALVE lowers both.

Update – August 9, 2016

The SALVE goal: Cc/Cs correction down to 20 kV
The prototype described above was a Cs-corrected, monochromated TEM and only a step on the way. The goal of SALVE was a TEM that corrects both Cs and Cc down to 20 kV. After Carl Zeiss had left the project in 2014[32], CEOS, FEI (today Thermo Fisher Scientific) and Ulm put this Cc/Cs corrector into operation in the SALVE III microscope[29] (see SALVE Cc Correction Realized[33]). Its information limit lies between 76 pm at 80 kV and 139 pm at 20 kV. At 20 kV, Young’s fringes now reach far beyond the 240 pm of the prototype (Fig. 19), and at 30 kV single atoms of graphene and MoS2 are resolved in raw images[29].

Update – March 1, 2022

60 kV STEM with an advanced hexapole corrector
Ten years later, JEOL and CEOS showed how far a Cs-corrected scanning microscope gets at 60 kV without Cc correction[26]. Ryusuke Sagawa and colleagues at JEOL, with Thomas Riedel, Peter Hartel, Martin Linck, Stephan Uhlemann and Heiko Müller of CEOS, used a JEOL NEOARM with a cold field-emission gun, a standard medium-gap pole piece and the advanced two-hexapole corrector ASCOR from CEOS. Instead of making the flat area of the ronchigram as large as possible, they balanced the residual sixth-order three-lobe aberration D6 with a deliberately set fourth-order three-lobe aberration D4, and chose the aperture semi-angle from the chromatic aberration and the energy width of the source: 38 mrad at an energy spread of 0.34 eV.

In ADF-STEM images of silicon [112] at 60 kV, with a probe current of 16 pA, the authors report the 78 pm (444) reflections in the Fourier transform of a single scan and, after aligning and averaging 20 fast scans, the 73 pm spacings; a simulation for the same conditions shows the same spots. Single-layer MoS2 gave 93 pm, and single sulfur vacancies were distinguished in a line profile. A check of the published Fourier transform of the averaged image for this article shows that the 73 pm value holds (Fig. 20): all four 73 pm reflections stand five to six times the noise level above the background, whereas 95 % of pure noise spots stay below 3.4 times, and the reflections out to 104 pm stand 13 to 19 times above it. In the single scan, the 78 pm reflections reach only 2.3 times the noise level and do not stand out from it, so only the averaged 73 pm value is used here. The DELTA corrector of the Triple C forms three hexapole fields with three dodecapoles[25]; the ASCOR is a double-hexapole corrector. The new point has been added to Fig. 17 above as an open red diamond: at 60 kV, the double-hexapole corrector of 2022 reaches 73 pm, against 96 pm for the DELTA microscope in 2010[24], and lies just above the chromatic limit. This is still the state of the art in 2027: the JEOL atomic-resolution multi-dimensional TEM (ARMD-TEM) with cold field-emission gun, Wien-filter monochromator and probe corrector, built with CEOS, routinely delivers sub-Ångström resolution in scanning mode at 60 or 200 kV, as Heil et al. write with reference to this study[26],[34]. As noted above, a Cs-corrected STEM compares with a Cs-corrected TEM at about 20 kV higher voltage.

Download this news article as PDF – for reading on paper, taking notes or filing.

References
  1. Kaiser, U., Biskupek, J., Meyer, J. C., Leschner, J., Lechner, L., Rose, H., Stöger-Pollach, M., Khlobystov, A. N., Hartel, P., Müller, H., Haider, M., Eyhusen, S., & Benner, G. (2011). Transmission Electron Microscopy at 20 kV for Imaging and Spectroscopy. Ultramicroscopy, 111(8), 1239–1246. https://doi.org/10.1016/j.ultramic.2011.03.012

  2. Haider, M., Rose, H., Uhlemann, S., Schwan, E., Kabius, B., & Urban, K. (1998). A Spherical-Aberration-Corrected 200 kV Transmission Electron Microscope. Ultramicroscopy, 75(1), 53–60. https://doi.org/10.1016/S0304-3991(98)00048-5

  3. Kabius, B., Hartel, P., Haider, M., Müller, H., Uhlemann, S., Loebau, U., Zach, J., & Rose, H. (2009). First Application of Cc-Corrected Imaging for High-Resolution and Energy-Filtered TEM. Journal of Electron Microscopy, 58(3), 147–155. https://doi.org/10.1093/jmicro/dfp021

  4. Egerton, R. F., McLeod, R., Wang, F., & Malac, M. (2010). Basic Questions Related to Electron-Induced Sputtering in the TEM. Ultramicroscopy, 110(8), 991–997. https://doi.org/10.1016/j.ultramic.2009.11.003

  5. Rose, H. H. (2009). Future Trends in Aberration-Corrected Electron Microscopy. Philosophical Transactions of the Royal Society A, 367(1903), 3809–3823. https://doi.org/10.1098/rsta.2009.0062

  6. Wilska, A. P. (1964). Low-Voltage Electron Microscopy: A 6-kV Instrument. Journal of the Royal Microscopical Society, 83(1–2), 207–211. https://doi.org/10.1111/j.1365-2818.1964.tb00530.x

  7. Sawada, H., Sasaki, T., Hosokawa, F., Yuasa, S., Terao, M., Kawazoe, M., Nakamichi, T., Kaneyama, T., Kondo, Y., Kimoto, K., & Suenaga, K. (2010). Higher-Order Aberration Corrector for an Image-Forming System in a Transmission Electron Microscope. Ultramicroscopy, 110(8), 958–961. https://doi.org/10.1016/j.ultramic.2010.01.010

  8. Krivanek, O. L., Dellby, N., Murfitt, M. F., Chisholm, M. F., Pennycook, T. J., Suenaga, K., & Nicolosi, V. (2010). Gentle STEM: ADF Imaging and EELS at Low Primary Energies. Ultramicroscopy, 110(8), 935–945. https://doi.org/10.1016/j.ultramic.2010.02.007

  9. Geim, A. K., & Novoselov, K. S. (2007). The Rise of Graphene. Nature Materials, 6(3), 183–191. https://doi.org/10.1038/nmat1849

  10. Meyer, J. C., Kisielowski, C., Erni, R., Rossell, M. D., Crommie, M. F., & Zettl, A. (2008). Direct Imaging of Lattice Atoms and Topological Defects in Graphene Membranes. Nano Letters, 8(11), 3582–3586. https://doi.org/10.1021/nl801386m

  11. Stöger-Pollach, M. (2010). Low Voltage TEM: Influences on Electron Energy Loss Spectrometry Experiments. Micron, 41(6), 577–584. https://doi.org/10.1016/j.micron.2010.04.007

  12. Stöger-Pollach, M. (2008). Optical Properties and Bandgaps From Low Loss EELS: Pitfalls and Solutions. Micron, 39(8), 1092–1110. https://doi.org/10.1016/j.micron.2008.01.023

  13. Bell, D. C., Russo, C. J., & Benner, G. (2010). Sub-Ångstrom Low-Voltage Performance of a Monochromated, Aberration-Corrected Transmission Electron Microscope. Microscopy and Microanalysis, 16(4), 386–392. https://doi.org/10.1017/S1431927610093670

  14. Haider, M., Hartel, P., Müller, H., Uhlemann, S., & Zach, J. (2010). Information Transfer in a TEM Corrected for Spherical and Chromatic Aberration. Microscopy and Microanalysis, 16(4), 393–408. https://doi.org/10.1017/S1431927610013498

  15. Suenaga, K., Sato, Y., Liu, Z., Kataura, H., Okazaki, T., Kimoto, K., Sawada, H., Sasaki, T., Omoto, K., Tomita, T., Kaneyama, T., & Kondo, Y. (2009). Visualizing and Identifying Single Atoms Using Electron Energy-Loss Spectroscopy With Low Accelerating Voltage. Nature Chemistry, 1(5), 415–418. https://doi.org/10.1038/nchem.282

  16. Moss, D. J., Ghahramani, E., Sipe, J. E., & van Driel, H. M. (1990). Band-Structure Calculation of Dispersion and Anisotropy in χ(3) for Third-Harmonic Generation in Si, Ge, and GaAs. Physical Review B, 41(3), 1542–1560. https://doi.org/10.1103/PhysRevB.41.1542

  17. Stöger-Pollach, M., Laister, A., & Schattschneider, P. (2008). Treating Retardation Effects in Valence EELS Spectra for Kramers–Kronig Analysis. Ultramicroscopy, 108(5), 439–444. https://doi.org/10.1016/j.ultramic.2007.07.003

  18. Palik, E. D. (Ed.) (1985). Handbook of Optical Constants of Solids. Academic Press, Orlando.

  19. Barton, B., Jiang, B., Song, C., Specht, P., Calderon, H., & Kisielowski, C. (2012). Atomic Resolution Phase Contrast Imaging and In-Line Holography Using Variable Voltage and Dose Rate. Microscopy and Microanalysis, 18(5), 982–994 (received 11 November 2011). https://doi.org/10.1017/S1431927612001213

  20. Bell, D. C., Russo, C. J., & Kolmykov, D. V. (2012). 40 keV Atomic Resolution TEM. Ultramicroscopy, 114, 31–37 (available online 29 December 2011). https://doi.org/10.1016/j.ultramic.2011.12.001

  21. Krivanek, O. L., Chisholm, M. F., Dellby, N., & Murfitt, M. F. (2011). Atomic-Resolution STEM at Low Primary Energies. In S. J. Pennycook & P. D. Nellist (Eds.), Scanning Transmission Electron Microscopy (pp. 615–658). Springer, New York. https://doi.org/10.1007/978-1-4419-7200-2_15

  22. Dellby, N., Bacon, N. J., Hrncirik, P., Murfitt, M. F., Skone, G. S., Szilagyi, Z. S., & Krivanek, O. L. (2011). Dedicated STEM for 200 to 40 keV Operation. The European Physical Journal Applied Physics, 54(3), 33505. https://doi.org/10.1051/epjap/2011100429

  23. Suenaga, K., Iizumi, Y., & Okazaki, T. (2011). Single Atom Spectroscopy With Reduced Delocalization Effect Using a 30 kV-STEM. The European Physical Journal Applied Physics, 54(3), 33508. https://doi.org/10.1051/epjap/2011100414

  24. Sasaki, T., Sawada, H., Hosokawa, F., Kohno, Y., Tomita, T., Kaneyama, T., Kondo, Y., Kimoto, K., Sato, Y., & Suenaga, K. (2010). Performance of Low-Voltage STEM/TEM With Delta Corrector and Cold Field Emission Gun. Journal of Electron Microscopy, 59(S1), S7–S13. https://doi.org/10.1093/jmicro/dfq027

  25. Morishita, S., Mukai, M., Suenaga, K., & Sawada, H. (2016). Atomic Resolution Imaging at an Ultralow Accelerating Voltage by a Monochromatic Transmission Electron Microscope. Physical Review Letters, 117, 153004. https://doi.org/10.1103/PhysRevLett.117.153004

  26. Sagawa, R., Yasuhara, A., Hashiguchi, H., Naganuma, T., Tanba, S., Ishikawa, T., Riedel, T., Hartel, P., Linck, M., Uhlemann, S., Müller, H., & Sawada, H. (2022). Exploiting the Full Potential of the Advanced Two-Hexapole Corrector for STEM Exemplified at 60 kV. Ultramicroscopy, 233, 113440. https://doi.org/10.1016/j.ultramic.2021.113440

  27. Sasaki, T., Sawada, H., Hosokawa, F., Sato, Y., & Suenaga, K. (2014). Aberration-Corrected STEM/TEM Imaging at 15 kV. Ultramicroscopy, 145, 50–55. https://doi.org/10.1016/j.ultramic.2014.04.006

  28. Calderon, H. A., Kisielowski, C., Specht, P., Barton, B., Godinez-Salomon, F., & Solorza-Feria, O. (2014). Maintaining the Genuine Structure of 2D Materials and Catalytic Nanoparticles at Atomic Resolution. Micron, 68, 164–175. https://doi.org/10.1016/j.micron.2014.08.007

  29. Linck, M., Hartel, P., Uhlemann, S., Kahl, F., Müller, H., Zach, J., Haider, M., Niestadt, M., Bischoff, M., Biskupek, J., Lee, Z., Lehnert, T., Börrnert, F., Rose, H., & Kaiser, U. (2016). Chromatic Aberration Correction for Atomic Resolution TEM Imaging From 20 to 80 kV. Physical Review Letters, 117(7), 076101. https://doi.org/10.1103/PhysRevLett.117.076101

  30. Börrnert, F., & Kaiser, U. (2018). Chromatic- and Geometric-Aberration-Corrected TEM Imaging at 80 kV and 20 kV. Physical Review A, 98(2), 023861. https://doi.org/10.1103/PhysRevA.98.023861

  31. Leist, C., Makurat, M., Jiao, A., Liu, X., Schneider, G. F., & Kaiser, U. (2025). Control of Grain Boundary Formation in Atomically Resolved Nanocrystalline Carbon Monolayers: Dependence on Electron Energy. Microscopy and Microanalysis, 31(1), ozae101. https://doi.org/10.1093/mam/ozae101

  32. SALVE news (2014). ZEISS Leaves SALVE. salve-project.de, February 6, 2014. https://salve-project.de/newspress/zeiss-leaves-salve-project.html

  33. SALVE news (2016). SALVE Cc Correction Realized. salve-project.de, August 9, 2016. https://salve-project.de/newspress/SALVE-CC-correction-realized.html

  34. Heil, T., Müller, H., Uhlemann, S., Linck, M., Löbau, U., Guzzinati, G., Kükelhan, P., Lörks, D., Elibol, K., Wang, H., Nakamura, A., Mukai, M., & van Aken, P. A. (2027). Pushing the Limits of Energy Resolution by Combining Monochromated EELS With the CEOS Energy-Filtering and Imaging Device in the JEOL Atomic-Resolution Multi-Dimensional TEM. Ultramicroscopy, 288, 114449. https://doi.org/10.1016/j.ultramic.2026.114449