Heating Oxo-Graphene

June 30, 2017 – Heating usually ruins the carbon lattice of graphene oxide. Researchers from Erlangen, Berlin, Ulm and the IFW Dresden have shown that oxo-functionalized graphene with oxo groups on only 4–6 % of its carbon atoms survives 270 °C largely intact: AC-HRTEM at 80 kV in Ulm imaged graphene areas 3–5 nm across, vacancies of a few atoms and some holes, about 0.8 % defects in all. A comparison with the TEAM 0.5 in Berkeley, the JEOL 2200MCO in Oxford and the Nion UltraSTEM 100 in Vienna shows that the chemistry, not the microscope, decides how much lattice survives.

Heating is the simplest way to turn graphene oxide back into graphene, and the worst: the oxygen leaves as carbon dioxide and takes carbon atoms with it, leaving a ruptured, undefined lattice. Researchers from Friedrich-Alexander-Universität Erlangen-Nürnberg, Freie Universität Berlin, Ulm University and IFW Dresden have now heated a gentler starting material, oxo-functionalized graphene (oxo-G), and looked at the result atom by atom with aberration-corrected high-resolution transmission electron microscopy (AC-HRTEM) at 80 kV in Ulm. Instead of amorphous carbon, they found a largely intact graphene lattice with only about 0.8 % defects. The box “Validation: FEI Titan at 80 kV vs. TEAM 0.5, JEOL 2200MCO and Nion UltraSTEM 100” below compares the images with those of three other microscopes at 60 and 80 kV.

Graphene from a flask
More than a decade after the first experiments with graphene[1], the chemical routes to it start either by reducing or by oxidizing graphite, and oxidation is favoured for producing large amounts of single-layer flakes[2],[3]. The best-known product is graphene oxide (GO). It carries mainly hydroxyl and epoxy groups on both sides of the carbon framework, but also many defects[3]. Defects caused by over-oxidation are permanent: without a carbon source, heating cannot heal them[4]. Many reducing agents remove the oxygen groups efficiently, but the agents themselves are often hard to remove[5]; for clean surfaces, the Erlangen team had shortly before reported a photochemical route[6].

Heating is convenient, but it adds many lattice defects[5],[7]. HRTEM of GO heated to 160 °C revealed an amorphous carbon lattice[8], and thermogravimetric analysis proved that CO and CO2 form. The process was not understood, and it was believed that graphene cannot be obtained this way.

A gentler starting material
Oxo-G differs from GO in one decisive point: its hexagonal carbon lattice is almost intact, and the oxo groups sit on it only as addends[2]. Standard oxo-G carries functional groups on about 50 % of its carbon atoms, and after chemical reduction its density of lattice defects is as low as about 0.03 %. For this study, the team started from graphite sulfate, in which sulfuric acid fills every gap between the graphite layers[9]. Adding water turned it into hydroxyl-functionalized graphite with groups on only about 4–6 % of the carbon atoms, called oxo-G4%, roughly one hydroxyl group per 24 carbon atoms. Single layers of it were drawn onto TEM grids as Langmuir–Blodgett films, as described in the box below.

The authors considered two paths for what heat does to this material (Fig. 1). In path I, oxo-G disproportionates: the carbon lattice sheds its groups and becomes graphene, while the oxo species turn mobile and may etch existing defects into holes a few nanometres across. In path II, the groups leave as CO2 and take lattice carbon with them, so new in-plane defects form.

▸ Recipe: oxo-G films for the TEM

Before and after 270 °C
Before heating, the HRTEM images showed clean and intact graphene areas about 5–10 nm across, next to some contamination and a few point defects (Fig. 2a). The inset, the Fourier transform of the image (its diffractogram), showed sharp spots of the intact hexagonal lattice. The hydroxyl groups themselves are not seen: they are very likely cleaved off by the electron beam, as the Erlangen team had shown before[11]. Next, a coated grid was heated to 270 °C in an activated-carbon bath, a method developed in Ulm to clean graphene of contamination[10]. At this temperature, the authors expected defects and an amorphous carbon framework, as had been found for oxo-G with about 50 % groups and for GO[5],[7].

Instead, the image after heating “reveals a surprisingly intact hexagonal carbon lattice”, the authors write (Fig. 2b). The spots in the diffractogram stayed distinct, “only slightly blurred due to some isotropic strain around the defects”. Point defects, mainly vacancies of a few atoms, appeared, together with some larger holes that were barely present before. The intact graphene areas measured up to 3–5 nm. Fig. 3 shows such a region at higher magnification: single and few-atom vacancies appear as small light-grey spots, mainly on the left, a hole at the upper right, and an area about 3 nm across is free of defects. Overviews of larger areas before and after heating, and the settings of the microscope, are in the box below (Fig. 4).

▸ Instruments and samples

Counting the defects
Raman spectroscopy, which probes the vibrations of the lattice with laser light, gave the numbers. On heated oxo-G4%, statistical Raman spectroscopy over many spots found a width of the 2D peak of Γ2D = 54 ± 14 cm−1 and a ratio of the defect-induced D peak to the G peak of ID/IG = 2.0 ± 0.2. By the relation of Lucchese, Cançado and co-workers[12],[13], this means an average distance between defects of about 3–4 nm, the size of the intact areas in the images. Spectra taken while heating from 25 to 500 °C showed that graphene starts to form at 75 °C and keeps forming up to 120 °C; above 250–300 °C its quality drops again, possibly because impurities react with the lattice. After heating to 175 °C, the 2D peak narrowed to 50 cm−1, a clear sign of graphene.

Before heating, chemical reduction had shown only about 0.03 % defects in oxo-G4%, one defect per about 3000 carbon atoms, so the defects seen after heating were made by the heat. With at least 4 % hydroxyl groups, one defect forms per about five groups removed. Since CO2 forms, the authors conclude that two hydroxyl groups make one defect, while the other three become mobile on the surface and either leave or, more likely, enlarge point defects by forming CO or CO2. The result is a density of lattice defects of about 0.8 %.

The process is more general. For oxo-G with about 50 % groups, the ID/IG ratio cannot be used, because it levels off at defect densities of about 3 %; the team read the density from the integrated area of the G peak instead, a method it had calibrated before[14]. Chemically reduced, this material had about 0.5 % defects; after heating, about 2 %. Heating thus added only about 1.5 %, one defect per about 30 converted sp3 centres (hydroxyl and epoxy groups). Most groups therefore leave graphene behind (path I in Fig. 1), and mobile epoxy and hydroxyl groups make the holes between 75 and 120 °C.

Validation: FEI Titan at 80 kV vs. TEAM 0.5, JEOL 2200MCO and Nion UltraSTEM 100
Graphene oxide has been imaged atom by atom in other laboratories too, each with another microscope and after another chemical history: reduced in hydrazine and annealed at 550 °C with the TEAM 0.5 at 80 kV in Berkeley, heated to 700 °C inside the JEOL 2200MCO at 80 kV in Oxford, and in 2019 with the scanning Nion UltraSTEM 100 at 60 kV in Vienna. The box below compares them with the FEI Titan at 80 kV in Ulm (Fig. 5).

▸ Validation: FEI Titan at 80 kV vs. TEAM 0.5, JEOL 2200MCO and Nion UltraSTEM 100

Challenges named by the authors
The authors name several limits. The hydroxyl groups cannot be imaged, because the beam very likely cleaves them[11], and some contamination remains on the layers. The ID/IG ratio of Raman spectra levels off at defect densities of about 3 %, so higher densities had to be estimated from the area of the G peak, whose relation to the degree of functionalization is only approximately double-logarithmic, between 0.5 % and about 20 %[14]. The defect count per removed group rests on the assumption of a minimal functionalization of 4 %. Above 250–300 °C, the quality of the graphene drops again. And for conventional GO, the authors expect the same process in its hexagonal regions, but “due to the high concentration of lattice defects, already induced during preparation, the growth of an intact graphene lattice is not possible”.

Graphene from heat after all
The study shows that heating does not have to destroy the lattice. Oxo-G with few groups turns into graphene with a defect density of about 0.8 %, mainly vacancies of a few atoms spread statistically over the lattice, next to a few holes 1–3 nm across. “Oxo-G can even act as a precursor to graphene, which does not require a reducing agent to form a reasonable hexagonal lattice of graphene,” the authors conclude. Layers with a controlled number of defects next to an intact lattice could serve as membranes for gas sieving[19], for energy storage or for sensing, and heating avoids impurities from reducing agents. The atomic-resolution images were taken with the aberration-corrected FEI Titan 80-300 at 80 kV at Ulm University.

Resource:
Grote, F., Gruber, C., Börrnert, F., Kaiser, U., Eigler, S. (2017).
Thermal Disproportionation of Oxo-Functionalized Graphene.
Angew. Chem. Int. Ed. 56(31), 9222–9225.
https://doi.org/10.1002/anie.201704419

Update – January 5, 2018

The news article of June 30, 2017 ends above. Later work is listed below.

A review ends with these images
In their review of defects in graphene oxide as structural motifs, Feicht and Eigler from the Freie Universität Berlin close the section on vacancy defects with the Ulm images before and after heating (Fig. 2)[18]. The growth of holes “suggests that oxo-groups are mobile on the surface, an effect that results in the growth of vacancy defects, that can further grow to hole defects”. Next to it, they set the Ulm images of reduced graphene oxide from 2010 beside the nanocrystalline commercial material from Oxford (see the news article Reduced Graphene Oxide) and conclude: “After a decade of intense graphene oxide research, it is time to step ahead and consider defects in graphene oxide as structural motifs.”

Update – February 26, 2018

Why the synthesis works
Researchers from Erlangen, Berlin and Ulm found out why the wet-chemical synthesis of oxo-G so often fails: molecular dynamics simulations showed that oxidation and a well-ordered stacking of the graphite layers lower the friction of the sulfuric acid between them[20]. Starting from highly crystalline natural graphite, the team made graphene with lattice defects down to 0.02 %, and AC-HRTEM at 80 kV in Ulm again imaged its intact carbon lattice atom by atom (see the news article Graphene Synthesis Understood).

Download this news article as PDF – for reading on paper, taking notes or filing.

References
  1. Novoselov, K. S., Geim, A. K., Morozov, S. V., Jiang, D., Zhang, Y., Dubonos, S. V., Grigorieva, I. V., Firsov, A. A. (2004). Electric Field Effect in Atomically Thin Carbon Films. Science, 306, 666–669. https://doi.org/10.1126/science.1102896

  2. Eigler, S., Enzelberger‐Heim, M., Grimm, S., et al. (2013). Wet Chemical Synthesis of Graphene. Adv. Mater., 25, 3583–3587. https://doi.org/10.1002/adma.201300155

  3. Eigler, S., Hirsch, A. (2014). Chemistry With Graphene and Graphene Oxide—Challenges for Synthetic Chemists. Angew. Chem. Int. Ed., 53, 7720–7738. https://doi.org/10.1002/anie.201402780

  4. Grimm, S., Schweiger, M., Eigler, S., Zaumseil, J. (2016). High-Quality Reduced Graphene Oxide by CVD-Assisted Annealing. J. Phys. Chem. C, 120, 3036–3041. https://doi.org/10.1021/acs.jpcc.5b11598

  5. Eigler, S., Grimm, S., Enzelberger-Heim, M., Müller, P., Hirsch, A. (2013). Graphene Oxide: Efficiency of Reducing Agents. Chem. Commun., 49, 7391. https://doi.org/10.1039/c3cc43612h

  6. Flyunt, R., Knolle, W., Kahnt, A., Halbig, C. E., Lotnyk, A., Häupl, T., Prager, A., Eigler, S., Abel, B. (2016). High Quality Reduced Graphene Oxide Flakes by Fast Kinetically Controlled and Clean Indirect UV-Induced Radical Reduction. Nanoscale, 8, 7572–7579. https://doi.org/10.1039/C6NR00156D

  7. Eigler, S., Grimm, S., Hof, F., Hirsch, A. (2013). Graphene Oxide: A Stable Carbon Framework for Functionalization. Journal of Materials Chemistry A, 1, 11559. https://doi.org/10.1039/c3ta12975f

  8. Dave, S. H., Gong, C., Robertson, A. W., Warner, J. H., Grossman, J. C. (2016). Chemistry and Structure of Graphene Oxide via Direct Imaging. ACS Nano, 10, 7515–7522. https://doi.org/10.1021/acsnano.6b02391

  9. Eigler, S. (2015). Graphite Sulphate – A Precursor to Graphene. Chem. Commun., 51, 3162–3165. https://doi.org/10.1039/C4CC09381J

  10. Algara-Siller, G., Lehtinen, O., Turchanin, A., Kaiser, U. (2014). Dry-Cleaning of Graphene. Appl. Phys. Lett., 104, 153115. https://doi.org/10.1063/1.4871997

  11. Butz, B., Dolle, C., Halbig, C. E., Spiecker, E., Eigler, S. (2016). Highly Intact and Pure Oxo‐Functionalized Graphene: Synthesis and Electron‐Beam‐Induced Reduction. Angew. Chem. Int. Ed., 55, 15771–15774. https://doi.org/10.1002/anie.201608377

  12. Lucchese, M. M., Stavale, F., Ferreira, E. H. M., Vilani, C., Moutinho, M. V. O., Capaz, R. B., Achete, C. A., Jorio, A. (2010). Quantifying Ion-Induced Defects and Raman Relaxation Length in Graphene. Carbon, 48, 1592–1597. https://doi.org/10.1016/j.carbon.2009.12.057

  13. Cançado, L. G., Jorio, A., Ferreira, E. H. M., Stavale, F., Achete, C. A., Capaz, R. B., Moutinho, M. V. O., Lombardo, A., Kulmala, T. S., Ferrari, A. C. (2011). Quantifying Defects in Graphene via Raman Spectroscopy at Different Excitation Energies. Nano Lett., 11, 3190–3196. https://doi.org/10.1021/nl201432g

  14. Vecera, P., Eigler, S., Koleśnik-Gray, M., Krstić, V., Vierck, A., Maultzsch, J., Schäfer, R. A., Hauke, F., Hirsch, A. (2017). Degree of Functionalisation Dependence of Individual Raman Intensities in Covalent Graphene Derivatives. Sci. Rep., 7, 45165. https://doi.org/10.1038/srep45165

  15. Erickson, K., Erni, R., Lee, Z., Alem, N., Gannett, W., Zettl, A. (2010). Determination of the Local Chemical Structure of Graphene Oxide and Reduced Graphene Oxide. Adv. Mater., 22, 4467–4472. https://doi.org/10.1002/adma.201000732

  16. Hofer, C., Skákalová, V., Görlich, T., Tripathi, M., Mittelberger, A., Mangler, C., Monazam, M. R. A., Susi, T., Kotakoski, J., Meyer, J. C. (2019). Direct Imaging of Light-Element Impurities in Graphene Reveals Triple-Coordinated Oxygen. Nat. Commun., 10, 4570. https://doi.org/10.1038/s41467-019-12537-3

  17. SALVE news (2010). Reduced Graphene Oxide. salve-project.de, March 3, 2010. https://salve-project.de/newspress/reduced-graphene-oxide.html

  18. Feicht, P., Eigler, S. (2018). Defects in Graphene Oxide as Structural Motifs. ChemNanoMat, 4, 244–252. https://doi.org/10.1002/cnma.201700357

  19. Garaj, S., Hubbard, W., Reina, A., Kong, J., Branton, D., Golovchenko, J. A. (2010). Graphene as a Subnanometre trans-Electrode Membrane. Nature, 467, 190–193. https://doi.org/10.1038/nature09379

  20. SALVE news (2018). Graphene Synthesis Understood. salve-project.de, February 26, 2018. https://salve-project.de/newspress/graphene-synthesis-understood.html