Reduced Graphene Oxide
March 3, 2010 – AC-HRTEM at 80 kV in Ulm shows what the chemical route from graphite to graphene leaves behind. Single layers of reduced graphene oxide from Stuttgart consist of intact graphene islands 3–6 nm across, separated by flat clusters of carbon pentagons, hexagons and heptagons in which every atom keeps three neighbours, invisible to spectroscopy. Dislocations that move apart under the beam show that the sheets are still strained. An independent study in Berkeley with the TEAM 0.5 at 80 kV confirms the graphene islands and the holes.
Graphene can be made by the bucketful from graphite: oxidize it, let the oxidized layers fall apart in water, and remove the oxygen again. What this chemical detour leaves behind in the carbon lattice had been unknown. Researchers from the Max Planck Institute for Solid State Research in Stuttgart, Madrid and Ulm have now imaged single layers of reduced graphene oxide atom by atom with aberration-corrected high-resolution transmission electron microscopy (AC-HRTEM) at 80 kV. They found intact graphene islands a few nanometres across, separated by flat patches of carbon pentagons, hexagons and heptagons in which every atom is still bonded to three neighbours, a kind of defect that spectroscopy cannot see. A study from Berkeley with the TEAM 0.5 microscope, also at 80 kV, later checked the picture on reduced graphene oxide made by another route (see “Validation: FEI Titan at 80 kV vs. TEAM 0.5 at 80 kV” below).
Graphene by the bucketful
Since graphene was first isolated[1], it has been made by peeling graphite, by growth on silicon carbide[2] or on metals[3], and from graphite dispersed in organic solvents[4]. None of these routes easily gives large quantities of processable sheets. The reduction of graphite oxide is a cheap alternative that is easy to scale up[5]–[7]. In graphite oxide, the graphene layers carry epoxy and hydroxyl groups, which makes them fall apart in water. The resulting graphene oxide (GO) monolayers can be deposited at a chosen density on almost any substrate, for example as thin conductive films on solid or flexible supports[8]–[10].
Chemical reduction raises the conductivity of the almost insulating GO by up to four orders of magnitude[11]–[13]. Yet reduced graphene oxide (RGO) still conducts 10 to 100 times worse than pristine graphene[14],[15]. The usual explanation is residual functional groups that survive the reduction. Despite many spectroscopic[16]–[19] and microscopic[13],[20],[21] studies, the atomic structure of GO and RGO had not been determined, because both are partly amorphous. In the most popular model, GO consists of randomly distributed oxidized areas carrying the oxygen groups and non-oxidized regions in which most carbon atoms keep their sp2 bonding[18]. As in carbon nanotubes[22] and fullerenes[23], topological defects, rings with other than six atoms, should strongly change the electronic and mechanical properties of graphene, and might explain why RGO falls short of pristine graphene.
One layer out of a hundred holes
The team deposited GO sheets on holey carbon TEM grids by dipping them into the solution and reduced them in a hydrogen plasma, as described in the box below. About 1 % of the holes in the grid were covered with sheets (Fig. 1c). Single layers were found by electron diffraction: they show only one hexagonal pattern (Fig. 1b), with the intensity ratios known from single-layer graphene[24]. This hexagonal pattern already shows that the sheets have long-range orientational order, which the earlier models did not suggest. Few-layer regions, in contrast, always showed several hexagonal patterns (Fig. 1a): the layers lie on top of each other with random rotations (turbostratic stacking), unlike the AB stacking of graphite and of mechanically exfoliated few-layer graphene[24],[25]. Such stacking is typical of weakly interacting sheets and confirms that the layers were fully oxidized and separated.
Tilted by 60°, the sheets turned out to be much rougher than mechanically exfoliated graphene (Fig. 1d). Horizontal dark lines appear where the sheet runs parallel to the beam, a sign of local deformations by up to 30°. From this image alone, the wrinkles could stem from solution processing and drying, from stress or from defects; the atomic-resolution images show that the strongest deformations surround the extended defects.
A patchwork map
Fig. 2 shows a typical single layer at atomic resolution, with the different regions coloured in panel (b). The largest part consists of clean, well-crystallized graphene with a clearly visible hexagonal lattice (light grey). The visible crystalline areas are 3 to 6 nm across and cover about 60 % of the surface. As in mechanically exfoliated graphene, there are regions with carbon adsorbates and heavier trapped atoms[27],[28] (dark grey), here about 30 % of the area, and holes that grow under the beam (yellow). Unlike exfoliated graphene, however, the clean areas contain many topological defects. Isolated ones, single bond rotations or dislocation cores made of a pentagon–heptagon pair, are marked green; individual adatoms or substitutions red. Extended, clustered topological defects appear as quasi-amorphous single-layer carbon patches (blue). They cover about 5 % of the surface and are typically 1 to 2 nm in diameter. Since contamination prefers to stick to defects, and the membrane under it cannot be seen, the share of defective regions is most likely underestimated.
Despite these defects, the long-range orientational order is kept, both in the images and in the diffraction patterns. Could the beam have made the defects? At 80 keV, the electrons do not create defects in pristine graphene at any density relevant here[25]; prolonged irradiation rather relaxes defects through occasional bond rotations, which sometimes anneal a pentagon–heptagon pair, but never a whole cluster. The defects were not seen in any mechanically exfoliated sample, and some RGO and exfoliated samples were made from the same source graphite, so the defects were not there before. They are left by the oxidation and reduction.
Flat and fully bonded
The clustered defects, shown in Fig. 3, contain many pentagons, heptagons and rotated hexagons within a nanometre-sized area, and a few octagons. Nevertheless, every carbon atom in them is bonded to three neighbours in a flat sp2 configuration. Since these clusters never occur in exfoliated graphene, they are the remnants of the originally strongly oxidized areas: the reduction has turned them back into sp2 carbon, but not into the crystalline hexagonal lattice. Because the bonding is the same as in graphene, spectroscopic methods cannot tell them apart. In Fig. 3a, typical pentagons, hexagons and heptagons are marked; with the intensity in their centres as a guide, the rest of the structure can be traced. Fig. 3b shows a partly assigned cluster of carbon rings in no apparent order.
The separation into defective and crystalline areas agrees with the model of Lerf and co-workers[18], and with nuclear magnetic resonance (NMR) studies that place most carbon atoms with hydroxyl and epoxide groups in highly oxidized areas next to undisturbed graphitic regions[17]. The exact atomic configuration of the oxidized state stays open, but the images show that oxidation and reduction leave disordered carbon inclusions that join the crystalline areas seamlessly. How these observations compare with the model, the NMR data, theory and exfoliated graphene is summarized in the validation box further below.
Strain around the defects
Near the clusters, the graphene lattice can be strongly distorted. In-plane distortions show up as bends in the lattice rows (red dashed lines in Fig. 3b and Fig. 4c,d). Out-of-plane distortions show up as a shorter projected lattice spacing in one direction: a reduction by 10 %, from 246 to 220 pm, is often found (Fig. 3a), which means that the membrane is locally inclined by arccos(0.9) ≈ 25°. These distortions are limited to the areas right next to the clusters; the larger defect-free areas look undistorted. For a dislocation, where an extra row of hexagons begins (right in Fig. 3b), a relaxed model shows the strong local deformation such a defect causes (inset).
The isolated defects show that the sheets were strongly strained at some point and are still under considerable strain. Most of them are dislocation cores with a pentagon–heptagon pair, the usual result of plastic deformation. Fig. 4a,b shows a dislocation dipole of two such pairs, imaged 2 minutes apart: the pairs move apart and the dipole grows. The energy to overcome the migration barrier may come from the beam, but in crystalline graphene such pairs anneal[25]. That they separate here means there is still enough strain to favour separation. Some carbon rings are even strongly stretched (arrows in Fig. 4c).
Two larger defect clusters are outlined in Fig. 4d. In one of them, the defects line up like a grain boundary, as predicted by Car and co-workers[29]. Next to the clusters, small patches of hexagonal lattice, typically 1 nm across, are rotated against the main orientation (yellow dashed lines in Fig. 4c,d). They too probably come from the oxidation and reduction, which in this case formed a small graphene-like area inside the defect. Such a patch may be the hardest to anneal, since it is already hexagonal locally, only misaligned with its surroundings.
Validation: FEI Titan at 80 kV vs. TEAM 0.5 at 80 kV
Five months later, researchers from the University of California at Berkeley, Lawrence Berkeley National Laboratory and Empa in Dübendorf imaged graphene oxide and reduced graphene oxide with the monochromated, aberration-corrected TEAM 0.5 microscope, also at 80 kV[33]. Their material was reduced by another route, in hydrazine vapour and by annealing at 550 °C. The box below compares the two microscopes and shows both materials side by side (Fig. 5).
Challenges named by the authors
The authors name several limits. About 30 % of the area is covered by contamination, under which the membrane cannot be seen; since contamination sticks preferably to defects, the defect share is most likely underestimated. Without heating the grids to 185 °C before imaging, an amorphous contamination layer hid the structure entirely. A small percentage of atoms moved during the exposure and could not be assigned, and the central part of the dislocation in Fig. 3b was not stable under the beam. The exact atomic configuration of the oxidized state before reduction remains unclear, and the wrinkles seen in tilted sheets could in principle also come from processing, drying or stress.
Defects to remove or to use
A scenario emerges for the oxidation and reduction of graphene: oxidation forms isolated, highly oxidized areas a few nanometres in size, while at least about 60 % of the surface stays undisturbed. Reduction turns the oxidized areas back into sp2-bonded carbon networks that lack the perfect crystallinity of graphene. These clustered topological defects induce strain and in-plane and out-of-plane deformations in the surrounding sheet, and isolated dislocations may have formed as a result of that strain. “The effects of these defects will have to be taken into account for any comprehensive study of the properties of this material,” the authors write. “Finally knowledge of the defect structures may help to devise procedures to remove them or alternatively, may lead to novel applications that take specific advantage of their presence.” The images were taken with the aberration-corrected FEI Titan 80-300 at 80 kV at Ulm University.
Resource:
Gómez-Navarro, C., Meyer, J. C., Sundaram, R. S., Chuvilin, A., Kurasch, S., Burghard, M., Kern, K., Kaiser, U. (2010).
Atomic Structure of Reduced Graphene Oxide.
Nano Lett. 10(4), 1144–1148.
https://doi.org/10.1021/nl9031617
Update – March 1, 2011
The news article of March 3, 2010 ends above. Later work on the same kind of defects is listed below.
Graphene oxide before the reduction
With the same FEI Titan at 80 kV, Cs set to 20 µm and Scherzer defocus, researchers from Cosenza, Ulm, the Paul Scherrer Institute in Villigen, Trieste, Stuttgart, Madrid and the EPFL in Lausanne, among them Cristina Gómez-Navarro and Jannik Meyer, looked at the starting material: graphene oxide before any reduction[34]. Unfiltered single exposures showed small patches of clean, defect-free graphene, while most of the area was covered by adsorbates or functional groups with no obvious structure. The ordered and the functionalized areas alternate on a few-nanometre scale, the same two-phase picture as in reduced graphene oxide. The extended topological defects that are frequent in the reduced material did not show up.
Three complications stand in the way of an atom-by-atom map of the oxygen groups, the team writes: carbon, nitrogen and oxygen give almost the same contrast, contamination is hard to tell apart from functional groups, and baking, which cleans graphene, already reduces graphene oxide. The material is also changed by the beam: after about 108 e/nm2 the exposed area shrank and radial wrinkles appeared around it, so “TEM images of this material may not represent the original structure of GO”. Reduced graphene oxide, by contrast, can be baked clean, is stable under the beam and consists mostly of carbon, which is why the 2010 images could be read ring by ring. X-ray absorption spectra of the same suspended membranes confirmed that most carbon atoms remain sp2-bonded, with carbonyl, epoxide and hydroxyl groups on the plane (see the news article Graphene Oxide Membranes).
Update – March 9, 2011
The same rings made on purpose
A year later, researchers from Helsinki, Espoo and Ulm used the electron beam itself to turn pristine graphene step by step into a flat, single-layer network of randomly arranged carbon rings, imaged with AC-HRTEM at 80 and 100 kV[35]. Pentagons, heptagons and rotated hexagons, the same building blocks as in the clusters of reduced graphene oxide, formed the first two-dimensional amorphous carbon (see the news article From Graphene to 2D Amorphous Carbon).
Update – May 10, 2012
Bond rotations at 80 kV
At 80 kV, an Ulm-led team with the Max Planck Institute for Solid State Research in Stuttgart watched grain boundaries in graphene move by single bond rotations: small rotated grains shrank until perfect graphene was left[36]. This is the kind of beam-driven bond rotation that occasionally annealed pentagon–heptagon pairs in reduced graphene oxide (see the news article Grain Boundary Migration).
Update – February 11, 2014
From crystal to glass
Researchers from Vienna, Helsinki and Ulm followed the change from graphene to a two-dimensional carbon glass atom by atom with 100 kV AC-HRTEM[37]. First a vitreous network separated small crystallites, then it took over, a sequence that resembles the patchwork of crystalline islands and disordered clusters in reduced graphene oxide (see the news article Carbon Glass).
Update – May 5, 2015
Defects as a showcase for in situ TEM
In a perspective on in situ transmission electron microscopy, researchers from Northwestern University write that “in situ TEM structural characterization of these 2D materials is particularly appealing, given that the lattice itself and lattice defects can be observed using the ultrahigh spatial resolution of the Cs/Cc-TEM”[38]. Their example figure is taken from the review of defects in graphene cited above[30]: models and HRTEM images of reconstructed divacancies with pentagons, heptagons and octagons, recorded by Jannik Meyer, the same kinds of rings as in the clusters of reduced graphene oxide. As a stimulus still to be applied inside the microscope, they name mechanical strain, the force that pulled the dislocation pair in Fig. 4a,b apart.
Update – July 19, 2016
Nanocrystalline graphene oxide at 700 °C
Researchers from MIT and the University of Oxford imaged commercially available, highly oxidized graphene oxide that had not been reduced, with the aberration-corrected JEOL 2200MCO at 80 kV[39]. At room temperature, a layer of amorphous surface contaminants hid the lattice, and it came back when the samples cooled down again. Only in an in-situ heating holder above 500 °C did the atomic structure appear. At 700 °C, the single-layer regions turned out to be nanocrystalline: sp2 crystallites of on average about 2 nm2 are each rotated against their neighbours and separated by disordered boundaries, so that areas larger than about 100 nm2 look amorphous in their Fourier transforms (Fig. 4e,f). The crystallites did not grow with time at 700 °C or under the beam. As in Ulm, the team traces the disorder back to the chemistry: it “is likely introduced during the oxidation or washing process”.
Feicht and Eigler from the Freie Universität Berlin set the two studies side by side in one figure in their review of defects in graphene oxide[40], as Fig. 4 does above: the Ulm images of graphene oxide reduced in a hydrogen plasma show a distorted lattice with intact graphene areas and locally rearranged rings (Fig. 4a–d), while in the heavily oxidized commercial material, “there is no long-range crystallographic order of the carbon lattice and patches of a disordered carbon lattice are observed. Even crystalline areas with a hexagonal lattice of few nm in diameter are unfrequent” (Fig. 4e,f). How much of the graphene lattice survives thus depends on how the material was oxidized and treated.
Update – June 30, 2017
Oxo-graphene: a lattice that survives heating
Researchers from the Freie Universität Berlin and Ulm University took the opposite route to the heavily oxidized material: oxo-functionalized graphene (oxo-G) made by controlled oxidation, with oxo groups on only 4–6 % of the carbon atoms of a single layer[41]. HRTEM showed clean, intact graphene areas about 5–10 nm across with a few point defects before heating (Fig. 6a). Heating to 270 °C, which turns graphene oxide into an amorphous carbon framework, left “a surprisingly intact hexagonal carbon lattice” with graphene areas of up to 3–5 nm, vacancies of a few atoms and some holes a few nanometres across that were barely present before (Fig. 6b); the diffractogram was only slightly blurred “due to some isotropic strain around the defects”. Raman spectra put the average distance between defects at about 3–4 nm, close to the 3–6 nm islands found in 2010. The authors explain the holes by oxo species that become mobile on heating and etch existing defects. Feicht and Eigler end their review with these images and note that “no grain boundaries are found in oxo-functionalized graphene”[40].
Update – October 8, 2019
Oxygen atoms seen directly
In HRTEM at 80 kV, carbon and oxygen look almost alike, so the 2010 study could not tell which atoms in the defect clusters were oxygen. Scanning TEM can: in annular dark-field images heavier atoms appear brighter. Researchers from the University of Vienna and Tübingen, among them Jannik Meyer, imaged graphene oxide with the Nion UltraSTEM 100 at 60 kV[42]. Most oxygen atoms sat in the plane of the lattice, as pairs replacing two neighbouring carbon atoms (about 44 % of 59 configurations) or at the edges of vacancies (about 49 %), in reconstructions like those of carbon-only vacancies; only about 7 % replaced a single carbon atom and had three carbon neighbours (Fig. 7). Such configurations are stable and “would be difficult to remove, e.g. by thermal annealing”; they may “play an important role among the structural configurations in GO or reduced GO”, the authors write. Some atoms of the 2010 clusters may thus have been oxygen in the plane rather than carbon. Under the scanning beam, adsorbates shrank and the clean lattice grew: graphene oxide was reduced inside the microscope.
Download this news article as PDF – for reading on paper, taking notes or filing.
-
Novoselov, K. S., Jiang, D., Schedin, F., Booth, T. J., Khotkevich, V. V., Morozov, S. V., Geim, A. K. (2005). Two-Dimensional Atomic Crystals. Proc. Natl. Acad. Sci. USA, 102, 10451–10453. https://doi.org/10.1073/pnas.0502848102
-
Berger, C., Song, Z., Li, T., et al. (2004). Ultrathin Epitaxial Graphite: 2D Electron Gas Properties and a Route Toward Graphene-Based Nanoelectronics. J. Phys. Chem. B, 108, 19912–19916. https://doi.org/10.1021/jp040650f
-
Kim, K. S., Zhao, Y., Jang, H., Lee, S. Y., Kim, J. M., Kim, K. S., Ahn, J.-H., Kim, P., Choi, J.-Y., Hong, B. H. (2009). Large-Scale Pattern Growth of Graphene Films for Stretchable Transparent Electrodes. Nature, 457, 706–710. https://doi.org/10.1038/nature07719
-
Hernandez, Y., Nicolosi, V., Lotya, M., et al. (2008). High-Yield Production of Graphene by Liquid-Phase Exfoliation of Graphite. Nat. Nanotechnol., 3, 563–568. https://doi.org/10.1038/nnano.2008.215
-
Park, S., Ruoff, R. S. (2009). Chemical Methods for the Production of Graphenes. Nat. Nanotechnol., 4, 217–224. https://doi.org/10.1038/nnano.2009.58
-
Stankovich, S., Dikin, D. A., Dommett, G. H. B., Kohlhaas, K. M., Zimney, E. J., Stach, E. A., Piner, R. D., Nguyen, S. T., Ruoff, R. S. (2006). Graphene-Based Composite Materials. Nature, 442, 282–286. https://doi.org/10.1038/nature04969
-
Stankovich, S., Piner, R. D., Chen, X., Wu, N., Nguyen, S. T., Ruoff, R. S. (2006). Stable Aqueous Dispersions of Graphitic Nanoplatelets via the Reduction of Exfoliated Graphite Oxide in the Presence of Poly(sodium 4-Styrenesulfonate). J. Mater. Chem., 16, 155–158. https://doi.org/10.1039/B512799H
-
Wang, X., Zhi, L., Müllen, K. (2007). Transparent, Conductive Graphene Electrodes for Dye-Sensitized Solar Cells. Nano Lett., 8, 323–327. https://doi.org/10.1021/nl072838r
-
Eda, G., Fanchini, G., Chhowalla, M. (2008). Large-Area Ultrathin Films of Reduced Graphene Oxide as a Transparent and Flexible Electronic Material. Nat. Nanotechnol., 3, 270–274. https://doi.org/10.1038/nnano.2008.83
-
Li, D., Müller, M. B., Gilje, S., Kaner, R. B., Wallace, G. G. (2008). Processable Aqueous Dispersions of Graphene Nanosheets. Nat. Nanotechnol., 3, 101–105. https://doi.org/10.1038/nnano.2007.451
-
Jung, I., Dikin, D. A., Piner, R. D., Ruoff, R. S. (2008). Tunable Electrical Conductivity of Individual Graphene Oxide Sheets Reduced at “Low” Temperatures. Nano Lett., 8, 4283–4287. https://doi.org/10.1021/nl8019938
-
Gilje, S., Han, S., Wang, M., Wang, K. L., Kaner, R. B. (2007). A Chemical Route to Graphene for Device Applications. Nano Lett., 7, 3394–3398. https://doi.org/10.1021/nl0717715
-
Gómez-Navarro, C., Weitz, R. T., Bittner, A. M., Scolari, M., Mews, A., Burghard, M., Kern, K. (2007). Electronic Transport Properties of Individual Chemically Reduced Graphene Oxide Sheets. Nano Lett., 7, 3499–3503. https://doi.org/10.1021/nl072090c
-
López, V., Sundaram, R. S., Gómez-Navarro, C., Olea, D., Burghard, M., Gómez-Herrero, J., Zamora, F., Kern, K. (2009). Chemical Vapor Deposition Repair of Graphene Oxide: A Route to Highly-Conductive Graphene Monolayers. Adv. Mater., 21, 4683–4686. https://doi.org/10.1002/adma.200901582
-
Tung, V. C., Allen, M. J., Yang, Y., Kaner, R. B. (2008). High-Throughput Solution Processing of Large-Scale Graphene. Nat. Nanotechnol., 4, 25–29. https://doi.org/10.1038/nnano.2008.329
-
Szabó, T., Berkesi, O., Forgó, P., Josepovits, K., Sanakis, Y., Petridis, D., Dékány, I. (2006). Evolution of Surface Functional Groups in a Series of Progressively Oxidized Graphite Oxides. Chem. Mater., 18, 2740–2749. https://doi.org/10.1021/cm060258+
-
Cai, W., Piner, R. D., Stadermann, F. J., et al. (2008). Synthesis and Solid-State NMR Structural Characterization of 13 C-Labeled Graphite Oxide. Science, 321, 1815–1817. https://doi.org/10.1126/science.1162369
-
Lerf, A., He, H., Forster, M., Klinowski, J. (1998). Structure of Graphite Oxide Revisited. J. Phys. Chem. B, 102, 4477–4482. https://doi.org/10.1021/jp9731821
-
Kudin, K. N., Ozbas, B., Schniepp, H. C., Prud'homme, R. K., Aksay, I. A., Car, R. (2007). Raman Spectra of Graphite Oxide and Functionalized Graphene Sheets. Nano Lett., 8, 36–41. https://doi.org/10.1021/nl071822y
-
Pandey, D., Reifenberger, R., Piner, R. (2008). Scanning Probe Microscopy Study of Exfoliated Oxidized Graphene Sheets. Surf. Sci., 602, 1607–1613. https://doi.org/10.1016/j.susc.2008.02.025
-
Mkhoyan, K. A., Contryman, A. W., Silcox, J., Stewart, D. A., Eda, G., Mattevi, C., Miller, S., Chhowalla, M. (2009). Atomic and Electronic Structure of Graphene-Oxide. Nano Lett., 9, 1058–1063. https://doi.org/10.1021/nl8034256
-
Gómez-Navarro, C., Pablo, P. J. D., Gómez-Herrero, J., Biel, B., Garcia-Vidal, F. J., Rubio, A., Flores, F. (2005). Tuning the Conductance of Single-Walled Carbon Nanotubes by Ion Irradiation in the Anderson Localization Regime. Nat. Mater., 4, 534–539. https://doi.org/10.1038/nmat1414
-
Saito, R., Dresselhaus, G., Dresselhaus, M. S. (1992). Topological Defects in Large Fullerenes. Chem. Phys. Lett., 195, 537–542. https://doi.org/10.1016/0009-2614(92)85559-S
-
Meyer, J. C., Geim, A. K., Katsnelson, M. I., Novoselov, K. S., Booth, T. J., Roth, S. (2007). The Structure of Suspended Graphene Sheets. Nature, 446, 60–63. https://doi.org/10.1038/nature05545
-
Meyer, J. C., Kisielowski, C., Erni, R., Rossell, M. D., Crommie, M. F., Zettl, A. (2008). Direct Imaging of Lattice Atoms and Topological Defects in Graphene Membranes. Nano Lett., 8, 3582–3586. https://doi.org/10.1021/nl801386m
-
Hummers, W. S., Offeman, R. E. (1958). Preparation of Graphitic Oxide. J. Am. Chem. Soc., 80, 1339. https://doi.org/10.1021/ja01539a017
-
Gass, M. H., Bangert, U., Bleloch, A. L., Wang, P., Nair, R. R., Geim, A. K. (2008). Free-Standing Graphene at Atomic Resolution. Nat. Nanotechnol., 3, 676–681. https://doi.org/10.1038/nnano.2008.280
-
Meyer, J. C., Girit, C. O., Crommie, M. F., Zettl, A. (2008). Imaging and Dynamics of Light Atoms and Molecules on Graphene. Nature, 454, 319–322. https://doi.org/10.1038/nature07094
-
Li, J.-L., Kudin, K. N., McAllister, M. J., Prud’homme, R. K., Aksay, I. A., Car, R. (2006). Oxygen-Driven Unzipping of Graphitic Materials. Phys. Rev. Lett., 96, 176101. https://doi.org/10.1103/PhysRevLett.96.176101
-
Banhart, F., Kotakoski, J., Krasheninnikov, A. V. (2011). Structural Defects in Graphene. ACS Nano, 5, 26–41 (available online 23 November 2010). https://doi.org/10.1021/nn102598m
-
Yakobson, B. I., Ding, F. (2011). Observational Geology of Graphene, at the Nanoscale. ACS Nano, 5, 1569–1574. https://doi.org/10.1021/nn200832y
-
Pantelic, R. S., Meyer, J. C., Kaiser, U., Stahlberg, H. (2012). The Application of Graphene as a Sample Support in Transmission Electron Microscopy. Solid State Commun., 152, 1375–1382. https://doi.org/10.1016/j.ssc.2012.04.038
-
Erickson, K., Erni, R., Lee, Z., Alem, N., Gannett, W., Zettl, A. (2010). Determination of the Local Chemical Structure of Graphene Oxide and Reduced Graphene Oxide. Adv. Mater., 22, 4467–4472. https://doi.org/10.1002/adma.201000732
-
Pacilé, D., Meyer, J. C., Fraile Rodríguez, A., Papagno, M., Gómez-Navarro, C., Sundaram, R. S., Burghard, M., Kern, K., Carbone, C., Kaiser, U. (2011). Electronic Properties and Atomic Structure of Graphene Oxide Membranes. Carbon, 49, 966–972. https://doi.org/10.1016/j.carbon.2010.09.063
-
SALVE news (2011). From Graphene to 2D Amorphous Carbon. salve-project.de, March 9, 2011. https://salve-project.de/newspress/from-graphene-to-two-dimensional-amorphous-carbon.html
-
SALVE news (2012). Grain Boundary Migration. salve-project.de, May 10, 2012. https://salve-project.de/newspress/grain-boundary-migration-in-graphene.html
-
SALVE news (2014). Carbon Glass. salve-project.de, February 11, 2014. https://salve-project.de/newspress/carbon-glass.html
-
Ramachandramoorthy, R., Bernal, R., Espinosa, H. D. (2015). Pushing the Envelope of In Situ Transmission Electron Microscopy. ACS Nano, 9, 4675–4685. https://doi.org/10.1021/acsnano.5b01391
-
Dave, S. H., Gong, C., Robertson, A. W., Warner, J. H., Grossman, J. C. (2016). Chemistry and Structure of Graphene Oxide via Direct Imaging. ACS Nano, 10, 7515–7522. https://doi.org/10.1021/acsnano.6b02391
-
Feicht, P., Eigler, S. (2018). Defects in Graphene Oxide as Structural Motifs. ChemNanoMat, 4, 244–252. https://doi.org/10.1002/cnma.201700357
-
Grote, F., Gruber, C., Börrnert, F., Kaiser, U., Eigler, S. (2017). Thermal Disproportionation of Oxo-Functionalized Graphene. Angew. Chem. Int. Ed., 56, 9222–9225. https://doi.org/10.1002/anie.201704419
-
Hofer, C., Skákalová, V., Görlich, T., Tripathi, M., Mittelberger, A., Mangler, C., Monazam, M. R. A., Susi, T., Kotakoski, J., Meyer, J. C. (2019). Direct Imaging of Light-Element Impurities in Graphene Reveals Triple-Coordinated Oxygen. Nat. Commun., 10, 4570. https://doi.org/10.1038/s41467-019-12537-3