Proton-Selective Graphene

November 27, 2025 – Graphene lets protons through but blocks methanol, which makes it a candidate membrane for methanol fuel cells. Researchers from Leiden, Ulm, Dresden, Darmstadt and Beijing grafted sulfophenyl groups onto centimeter-sized single-crystal graphene; the membrane doubled the fuel-cell power of Nafion™. Aberration-corrected HRTEM at 80 kV with the SALVE microscope showed that the lattice stayed free of holes in all three batches. In the supplementary HRTEM images shown here (about 15 pixels per nm, one pixel ≈ 0.67 Å), the finest lattice spacing resolved is 1.72 Å, in a small crystallite.

A perfect fuel-cell membrane would be a sieve that only protons can pass. In a direct methanol fuel cell, protons must travel quickly from anode to cathode, while the methanol fuel must stay behind, because any methanol that leaks across poisons the catalyst and wastes fuel. Graphene, a single layer of carbon atoms, is impermeable to water and other molecules yet lets a small number of protons through, mainly at defects: defect-free regions are practically closed to them[1],[2]. Researchers from Leiden University (the Netherlands), Ulm University, TU Darmstadt, TU Dresden, CASUS and Helmholtz-Zentrum Dresden-Rossendorf (Germany), Peking University and the Beijing Graphene Institute (China) have now grafted sulfophenyl groups onto centimeter-sized single-crystal graphene to open proton paths without punching holes. Aberration-corrected HRTEM with the SALVE microscope in Ulm checked that the lattice stayed closed.

Ulm had shown before what lattice defects do: in carbon films full of eight-membered rings, imaged by HRTEM, protons pass about 1000 times more easily than through perfect graphene, while helium stays blocked[3]. Here the lattice is not rebuilt but decorated, so the question for the microscope is a different one: does the chemistry leave the honeycomb intact?

Sulfophenyl groups as proton shuttles
The team used a diazonium reaction[4] with 4-sulfobenzenediazonium (4-SBD). An electron from the graphene reduces the 4-SBD cation, which releases N2 and leaves an aryl radical that binds perpendicular to the lattice. The carbon atom underneath switches from flat sp2 to tetrahedral sp3 bonding, and the site carries the negative charge of the sulfonate and an out-of-plane dipole. 4-SBD can also attack an aryl group that is already grafted, so that oligomers of aryl groups grow on the graphene[5].

Density functional theory (DFT) on circumcoronene, a small flake of graphene, shows why such a site helps a proton across. The grafted groups stretch the neighbouring hexagonal rings, up to 6.8 % for a ring with sulfophenyl groups on both sides, and lower the energy barrier. Phenyl or sulfophenyl groups on both sides raised the calculated proton flux by eight to nine orders of magnitude, hydrogenation only by one. A distorted ring, however, is exactly what the reaction must create without opening a pore.

Single-crystal graphene on the TEM grid
To keep defects and grain boundaries to a minimum, the team used centimeter-sized single-crystal CVD graphene whose domains were seamlessly stitched together in alignment[6]. Selected-area electron diffraction (JEOL JEM-2100 at 200 kV) at several positions across a suspended film gave patterns with the same orientation, so the film is one crystal, and the intensity profile of the reflections identified it as a monolayer. For the microscope the graphene was transferred without any polymer: a TEM grid was set on the graphene side of the copper foil, the copper was etched away in ammonium persulfate solution, and the free-standing graphene was rinsed three times in ultrapure water. The graphene on the Quantifoil grid was then incubated with 4-SBD (1 mg·ml−1 in 0.1 M HCl) for up to six days.

SALVE at 80 kV: no holes in the lattice
Christopher Leist, Haoyuan Qi, Xinliang Feng and Ute Kaiser contributed the HRTEM characterization. The images were taken with the SALVE microscope, whose image-side corrector removes both chromatic (CC) and spherical (CS) aberration, at 80 kV with a resolution of 76 pm, recorded on a Ceta CMOS camera[7]. After four and six days of treatment, the HRTEM images show the graphene lattice running on over large areas between patches of adsorbed material (Fig. 1). Not a single pore larger than 1 nm appeared. Lower-magnification TEM images of the film suspended over the holes of the grid, with electron diffraction of the circled areas, show the graphene reflections at 2.1 Å before the treatment and still after four and six days (Fig. 2).

To make sure this was no lucky area, all three batches of 4-SBD used in the study were imaged: batch 2 day by day from one to six days of treatment (Fig. 3), batch 3 after two and four days (Fig. 4). In none of them did the treatment create vacancy-like defects. The reaction thus decorates the lattice without punching holes into it, which is the condition for a membrane that lets protons through but no methanol.

How much of the lattice is covered can be read from the same colour maps: the share of each field tinted orange (Table 1). The paper itself gives no such number, so it was measured for this article. Coverage ranges from 12 to 63 % and does not rise steadily with treatment time; the least covered field is batch 2 after five days (12 %, Fig. 3e), the most covered batch 3 after four days (63 %, Fig. 4b). Each value comes from a single field of 15 nm × 15 nm (Fig. 1: about 20 nm × 16 nm), so it describes that spot rather than the whole membrane, and HRTEM cannot tell oligomerized 4-SBD from the hydrocarbon contamination that CVD graphene carries anyway. What all fields share is the clean lattice between the patches, without holes.

Sample4-SBD treatmentImageFieldCovered
Paper Fig. 2E4 daysFig. 1a20 × 16 nm44 %
Paper Fig. 2E6 daysFig. 1b20 × 16 nm56 %
Batch 21 dayFig. 3a15 × 15 nm34 %
Batch 22 daysFig. 3b15 × 15 nm43 %
Batch 23 daysFig. 3c15 × 15 nm51 %
Batch 24 daysFig. 3d15 × 15 nm50 %
Batch 25 daysFig. 3e15 × 15 nm12 %
Batch 26 daysFig. 3f15 × 15 nm47 %
Batch 32 daysFig. 4a15 × 15 nm58 %
Batch 34 daysFig. 4b15 × 15 nm63 %

Table 1: Share of each HRTEM field covered by adsorbed material, measured for this article on the colour maps of Figs. 1, 3 and 4 (area where the graphene lattice reflections are weak against the disordered 0.35–1 nm contrast). Covered = orange plus the violet crystallites in Fig. 3a (about 3 % of that field); the green areas there, possibly bilayer, count as clean graphene. One field per entry; 4-SBD oligomers and hydrocarbon contamination are not distinguished.

The images also show where HRTEM reaches its limits on this sample. Individual grafting sites could not be resolved on the monolayer regions, and no expansion of the lattice from the sp3 distortions was visible. The oligomers of 4-SBD could not be told apart from the common hydrocarbon contamination that CVD graphene carries from its growth and transfer. Whether sulfophenylation seals grain boundaries or defects also remained beyond what the images showed.

A membrane that beats Nafion™
In the fuel cell, graphene treated for four days delivered a maximum power density of 109.8 ± 14.8 mW·cm−2, about twice that of the standard polymer membrane Nafion™ 117. Raising the methanol concentration from 1 M to 5 M cut the power of the Nafion™ cell by about 53 %, but that of the graphene cell by only about 10 %. Longer treatment did not help, since the oligomers then block the proton paths again. “These findings propose functionalized graphene as an alternative to polymer membranes for electrochemical energy devices,” the authors write. Molecular dynamics simulations in the paper (ReaxFF with metadynamics) show how a grafted group can help: its sulfonate captures a proton from the water with a barrier of about 0.15–0.20 eV, passes it down along the phenyl ring and releases it about 3 Å above the basal plane, from where it can tunnel through the distorted lattice (Fig. 5). What exactly drives the gain, sp3 distortions or the functional groups at the graphene–electrolyte interface, still needs to be pinned down; resolving single grafting sites in the lattice would be the next task for the microscope.

Resource:
Zhang, W., Makurat, M., Liu, X., Chen, B., Li, Y., Liu, X., Kock, T. J. F., Jiao, A., Jiang, G., Leist, C., Maheu, C., Sezen, H., Calvani, D., Eren, I., Jiang, L., Buda, F., Qi, H., Hofmann, J. P., Feng, X., Kaiser, U., Sun, L., Liu, Z., Kuc, A., Heine, T., & Schneider, G. F. (2025).
Sulfophenylated centimeter-sized graphene membrane in a direct methanol fuel cell.
Nat. Commun. 16, 10857.
https://doi.org/10.1038/s41467-025-65507-3

Download this news article as PDF – for reading on paper, taking notes or filing.

References
  1. Bentley, C. L., Kang, M., Bukola, S., Creager, S. E., & Unwin, P. R. (2022). High-Resolution Ion-Flux Imaging of Proton Transport Through Graphene/Nafion Membranes. ACS nano, 16(4), 5233-5245. https://doi.org/10.1021/acsnano.1c05872

  2. Achtyl, J. L., Unocic, R. R., Xu, L., Cai, Y., Raju, M., Zhang, W., Sacci, R. L., Vlassiouk, I. V., Fulvio, P. F., Ganesh, P., Weselowski, D. J., Dai, S., van Duin, A. C. T., Neurock, M., & Geiger, F. M. (2015). Aqueous Proton Transfer Across Single-Layer Graphene. Nature communications, 6(1), 6539. https://doi.org/10.1038/ncomms7539

  3. SALVE news (2020). Proton and Lithium Permeation Through Defective Graphene. salve-project.de, May 19, 2020. https://salve-project.de/newspress/proton_and_lithium_permeation_through_defective_graphene.html

  4. Park, J., & Yan, M. (2013). Covalent Functionalization of Graphene With Reactive Intermediates. Accounts of Chemical Research, 46(1), 181-189. https://doi.org/10.1021/ar300172h

  5. Mahouche-Chergui, S., Gam-Derouich, S., Mangeney, C., & Chehimi, M. M. (2011). Aryl Diazonium Salts: A New Class of Coupling Agents for Bonding Polymers, Biomacromolecules and Nanoparticles to Surfaces. Chemical Society Reviews, 40(7), 4143-4166. https://doi.org/10.1039/c0cs00179a

  6. Sun, L., Chen, B., Wang, W., Li, Y., Zeng, X., Liu, H., Liang, Y., Zhao, Z., Cai, A., Zhang, R., Zhu, Y., Wang, Y., Song, Y., Ding, Q., Gao, X., Peng, H., Li, Z., Lin, L., & Liu, Z. (2021). Toward Epitaxial Growth of Misorientation-Free Graphene on Cu (111) Foils. ACS nano, 16(1), 285-294. https://doi.org/10.1021/acsnano.1c06285

  7. Linck, M., Hartel, P., Uhlemann, S., Kahl, F., Müller, H., Zach, J., Haider, M., Niestadt, M., Bischoff, M., Biskupek, J., Lee, Z., Lehnert, T., Börrnert, F., Rose, H., & Kaiser, U. (2016). Chromatic Aberration Correction for Atomic Resolution TEM Imaging From 20 to 80 kV. Physical Review Letters, 117(7), 076101. https://doi.org/10.1103/physrevlett.117.076101