Patched Graphene from Glucose

August 21, 2012 – Researchers from the Max Planck Institute of Colloids and Interfaces in Potsdam-Golm and Ulm have made gram amounts of free-standing graphene from glucose, with a carbon nitride template that decomposes during the synthesis. Aberration-corrected HRTEM at 80 kV in Ulm shows a mosaic of graphene patches 2 to 15 nm across, joined by pentagon–heptagon grain boundaries: “patched” graphene, between ideal graphene and amorphous carbon.

Graphene can be baked from glucose. Researchers from the Max Planck Institute of Colloids and Interfaces in Potsdam-Golm and Ulm University heated sugar together with dicyandiamide, a cheap nitrogen compound, under nitrogen and obtained gram amounts of free-standing graphene sheets, without substrate, catalyst, solvent or vacuum. Aberration-corrected HRTEM at 80 kV in Ulm shows what these sheets are made of: not one large crystal, but a mosaic of graphene patches 2 to 15 nanometres across, joined along grain boundaries of five- and seven-membered rings. The authors call it “patched” graphene, a new form of two-dimensional carbon between ideal graphene and amorphous carbon.

Graphene from a crucible
High-quality graphene films are grown by chemical vapor deposition on metal foils[1],[2], which suits electronics but not the tonnes of graphene powder that batteries, catalysts and composites need. Powder is still made mostly by chemical exfoliation of graphite through graphite oxide[3]. Building graphene up from small molecules, as chemists do for nanoribbons on metal surfaces[4], has so far worked only on a substrate and in small amounts.

The Potsdam route uses a sacrificial template. Heated to 600 °C, dicyandiamide condenses into graphitic carbon nitride (g-C3N4), a layered material much like graphite[5]. The carbon from the glucose binds to the surfaces of its layers and condenses in the gaps between them, so it is forced to grow flat, one or a few layers thick[6]. Above 750 °C the carbon nitride decomposes completely and leaves the graphene sheets behind. At 1000 °C the product, called Gr, still contains 4.3 atom % nitrogen. The steps are given in the box below.

▸ Recipe: graphene from glucose

A mosaic of patches
The monoliths are extremely light, 0.0077 g/cm3, and consist of thin, crumpled sheets up to hundreds of micrometres in size. Mild ultrasound in dimethylformamide or water separates them into single flakes. In dark-field TEM images, the unfolded parts of these flakes have a homogeneous, very low thickness (Fig. 1a, b).

The aberration-corrected HRTEM images at 80 kV resolve the honeycomb of hexagonally bonded carbon atoms in these thin areas (Fig. 1c). The honeycomb, however, does not continue across the flake: it breaks up into domains between 2 and 15 nm across, each with its own lattice orientation, with irregular shapes and visible boundaries. Where two domains of a single layer meet, the boundary is built from pairs of pentagons and heptagons (black arrow in Fig. 1c), the same kind of grain boundary found in graphene grown by chemical vapor deposition and seen moving under the beam in Ulm[7].

The colour map of Fig. 2b makes the mosaic visible: every colour marks one domain with a single lattice orientation. Most of the area is single or double layer; thicker, multilayer domains (outlined in black) form only a small fraction. Because the patches are interconnected into a continuous sheet, the authors call the material nanocrystalline or patched graphene. A similar nanocrystalline graphene had been made shortly before in Bielefeld by annealing cross-linked aromatic monolayers on a substrate[8]; the glucose route makes it without substrate and by the gram.

Holes under the beam
Thin carbon of this kind is sensitive to the 80 keV electrons. During imaging, holes open in the sheet (white arrow in Fig. 1c) and grow, as the two supporting videos of the paper show (Video 1, Video 2). Such holes are typical for very thin carbon. Imaging at 80 kV with an aberration corrector keeps atomic contrast while limiting this damage, the approach used in Ulm for molecules reacting inside nanotubes[9] and for the transformation of graphene into two-dimensional amorphous carbon[10].

Video 1: AC-HRTEM video at 80 kV: a hole forms in the thin patched graphene under the electron beam (Movie S1 of the paper, slowed down 2.5 times).

Video 2: AC-HRTEM video at 80 kV: holes grow under continued irradiation (Movie S2 of the paper, slowed down 2.5 times).

Validation: HRTEM vs. bulk methods
HRTEM sees a few hundred square nanometres; the monolith weighs grams. The paper therefore tests the picture from the microscope against methods that average over the whole sample: Raman spectroscopy, X-ray photoelectron spectroscopy (XPS), X-ray diffraction and gas sorption. The comparison is in the box below.

▸ Validation: HRTEM vs. Raman, XPS and sorption

Tunable nitrogen
The same route sets the amount of nitrogen in the sheets. At 800 °C for one hour, sample NG1 contains 26.8 atom % nitrogen and conducts only 0.017 S/m, five orders of magnitude less than Gr; higher temperatures and longer times bring the nitrogen down step by step to the 4.3 atom % of Gr, while the morphology and the surface area stay the same. XPS shows that most nitrogen sits in pyridinic positions at the domain edges and part of it in graphitic positions inside the lattice: unlike annealing finished graphene in ammonia, which dopes mainly edges and defects, all samples hold more than 10 % graphitic nitrogen. This matters because the electronic properties of doped graphene depend strongly on the dopant concentration[12], which earlier methods controlled only poorly. The mass ratio of the two precursors sets the thickness: lowering it from 40 to 10 raises the average layer number from three to about eight.

Challenges named by the authors
The synthesis was not optimized for large plates; the domains stay small, 2 to 15 nm, and the sheets tear easily into flakes under ultrasound. Multilayer domains remain as a smaller fraction of the sample. The very high surface area makes the material a superadsorber: clean samples exist only in high vacuum, and in air gases and water are taken up at once, which also shows in the oxygen content measured by XPS. Under the electron beam, holes form and grow in the thin patches.

The recipe also has a lower limit. Below a mass ratio of about 10 between dicyandiamide and glucose, no layered flakes form, and at 5 or less the product is only a sponge-like, mesoporous graphitic carbon.

“Two-dimensional patched graphene can be understood as a novel species between ideal graphene and amorphous carbon,” the authors conclude. Made from sugar without solvents, catalysts, substrates or vacuum, it opens a way to mass production of conductive, nitrogen-tunable graphene for electrodes, catalysts and fillers.

Resource:
Li, X.-H., Kurasch, S., Kaiser, U., & Antonietti, M. (2012).
Synthesis of Monolayer-Patched Graphene from Glucose.
Angew. Chem. Int. Ed. 51(38), 9689–9692.
https://doi.org/10.1002/anie.201203207

Download this news article as PDF – for reading on paper, taking notes or filing.

References
  1. Li, X., Cai, W., An, J., Kim, S., Nah, J., Yang, D., Piner, R., Velamakanni, A., Jung, I., Tutuc, E., Banerjee, S. K., Colombo, L., Ruoff, R. S. (2009). Large-Area Synthesis of High-Quality and Uniform Graphene Films on Copper Foils. Science, 324, 1312–1314. https://doi.org/10.1126/science.1171245

  2. Kim, K. S., Zhao, Y., Jang, H., Lee, S. Y., Kim, J. M., Kim, K. S., Ahn, J., Kim, P., Choi, J., Hong, B. H. (2009). Large-Scale Pattern Growth of Graphene Films for Stretchable Transparent Electrodes. Nature, 457, 706–710. https://doi.org/10.1038/nature07719

  3. Park, S., Ruoff, R. S. (2009). Chemical Methods for the Production of Graphenes. Nat. Nanotechnol., 4, 217–224. https://doi.org/10.1038/nnano.2009.58

  4. Cai, J., Ruffieux, P., Jaafar, R., Bieri, M., Braun, T., Blankenburg, S., Muoth, M., Seitsonen, A. P., Saleh, M., Feng, X., Müllen, K., Fasel, R. (2010). Atomically Precise Bottom-Up Fabrication of Graphene Nanoribbons. Nature, 466, 470–473. https://doi.org/10.1038/nature09211

  5. Thomas, A., Fischer, A., Goettmann, F., Antonietti, M., Müller, J., Schlögl, R., Carlsson, J. M. (2008). Graphitic Carbon Nitride Materials: Variation of Structure and Morphology and Their Use as Metal-Free Catalysts. J. Mater. Chem., 18, 4893. https://doi.org/10.1039/b800274f

  6. Li, X., Chen, J., Wang, X., Sun, J., Antonietti, M. (2011). Metal-Free Activation of Dioxygen by Graphene/g-C3N4 Nanocomposites: Functional Dyads for Selective Oxidation of Saturated Hydrocarbons. J. Am. Chem. Soc., 133, 8074–8077. https://doi.org/10.1021/ja200997a

  7. SALVE news (2012). Grain Boundary Migration. salve-project.de, May 10, 2012. https://salve-project.de/newspress/grain-boundary-migration-in-graphene.html

  8. Turchanin, A., Weber, D., Büenfeld, M., Kisielowski, C., Fistul, M. V., Efetov, K. B., Weimann, T., Stosch, R., Mayer, J., Gölzhäuser, A. (2011). Conversion of Self-Assembled Monolayers Into Nanocrystalline Graphene: Structure and Electric Transport. ACS Nano, 5, 3896–3904. https://doi.org/10.1021/nn200297n

  9. Chuvilin, A., Bichoutskaia, E., Gimenez-Lopez, M. C., Chamberlain, T. W., Rance, G. A., Kuganathan, N., Biskupek, J., Kaiser, U., Khlobystov, A. N. (2011). Self-Assembly of a Sulphur-Terminated Graphene Nanoribbon Within a Single-Walled Carbon Nanotube. Nat. Mater., 10, 687–692. https://doi.org/10.1038/nmat3082

  10. Kotakoski, J., Krasheninnikov, A. V., Kaiser, U., Meyer, J. C. (2011). From Point Defects in Graphene to Two-Dimensional Amorphous Carbon. Phys. Rev. Lett., 106, 105505. https://doi.org/10.1103/PhysRevLett.106.105505

  11. Chen, Z., Ren, W., Gao, L., Liu, B., Pei, S., Cheng, H. (2011). Three-Dimensional Flexible and Conductive Interconnected Graphene Networks Grown by Chemical Vapour Deposition. Nat. Mater., 10, 424–428. https://doi.org/10.1038/nmat3001

  12. Zhao, L., He, R., Rim, K. T., Schiros, T., Kim, K. S., Zhou, H., Gutiérrez, C., Chockalingam, S. P., Arguello, C. J., Pálová, L., Nordlund, D., Hybertsen, M. S., Reichman, D. R., Heinz, T. F., Kim, P., Pinczuk, A., Flynn, G. W., Pasupathy, A. N. (2011). Visualizing Individual Nitrogen Dopants in Monolayer Graphene. Science, 333, 999–1003. https://doi.org/10.1126/science.1208759