Core-Loss EFTEM of Graphene

September 19, 2020 – Researchers at Ulm University, together with Harald Rose, have imaged graphene with electrons that lost about 300 eV at the carbon K edge, using the SALVE microscope at 80 kV, which is corrected for chromatic and spherical aberration. The core-loss images show the graphene lattice, but depending on the focus the carbon atoms appear bright or dark, just as in the elastic zero-loss and plasmon-loss images. Even for a single layer of light atoms, such images are therefore not a direct elemental map, in line with earlier findings on thicker crystals at the chromatic and spherical aberration corrected PICO microscope in Jülich at 80 to 300 kV.

An electron that kicks an inner-shell electron out of a carbon atom loses about 300 eV, and it carries that signature only because it met carbon. Filtering an image for such electrons should therefore show where the carbon atoms are: a chemical map with atomic resolution, each atom glowing like a small lamp. The team tested this promise on the simplest sample there is, a single layer of graphene, in a microscope corrected for both chromatic and spherical aberration. The carbon atoms did show up in the core-loss image. But depending on the focus, they appeared bright or dark, and so the image is not a direct map of where the carbon is.

Energy-filtered transmission electron microscopy (EFTEM) forms an image only from electrons that have lost a chosen amount of energy in the sample. Lenses focus electrons of different energy at different depths, and this chromatic aberration used to blur energy-filtered images far beyond atomic scale. Correcting it[1] made atomic resolution possible even for wide energy windows[2] and at voltages from 20 to 80 kV[3],[4]. With a corrected microscope, researchers in Jülich had already obtained lattice images from the silicon L2,3 edge of silicon[5] and from the titanium L2,3 and oxygen K edges of SrTiO3[6]. Both teams noticed that part of the contrast came from ordinary elastic scattering, since an electron that loses energy is usually also scattered elastically[7]. This elastic or phase contrast survives in the energy-filtered image[8]–[10]. Simulations nevertheless suggested that for samples thinner than a few nanometers, where electrons scatter only once, the core-loss image could still be read directly as an elemental map[6],[9],[10].

Graphene is the ideal test of this idea: one layer of light carbon atoms, so thin that multiple scattering hardly occurs. The team compared three filtered signals of the same areas: the zero-loss image, which is the familiar phase-contrast image; the plasmon-loss image at about 16 eV, whose inelastic scattering is spread far beyond an atom[11],[12] so that any lattice contrast in it must be preserved elastic contrast; and the image from the carbon K edge, where the inelastic scattering itself is localized enough to show atoms.

A thousand times the usual dose
The carbon K-edge signal is weak: it is only about one ten-thousandth of the elastic signal in the zero-loss peak (Fig. 1a). To collect enough electrons in a 20 eV window centered at 300 eV, the researchers needed about 109 electrons per nm2, roughly a thousand times the dose of a normal high-resolution image of graphene. Even so, the raw core-loss image shows no lattice, only a bright cloud of the focused beam and some carbon contamination at the edge (Fig. 1b). Its Fourier transform, however, clearly holds the first-order reflections of graphene (Fig. 1c). After one to two minutes the beam drilled nanometer-sized holes into the graphene, so only a few single exposures were possible. The researchers therefore averaged each image over more than 100 unit cells of the graphene lattice. The microscope settings are listed in the box below.

▸ Instruments and samples

Bright atoms or dark atoms
After averaging, the core-loss images show the graphene lattice. In one experiment, the carbon atoms appear bright in both the zero-loss and the K-edge image (Fig. 2a, b), the elastic image with a much stronger signal. At another focus, both images switch to dark atoms on a bright background (Fig. 2c, d). The researchers reproduced this at different places on the sample. In none of their experiments, the authors note, did the contrast differ between the zero-loss and the K-edge image.

A focus series made the effect systematic. Starting at the focus with the strongest lattice contrast, the team changed the defocus in 2 nm steps from −20 to +20 nm. Within only ±8 nm of the optimum, the K-edge contrast switched several times between dark and bright atoms (Fig. 3a); further out the lattice vanished. Image simulations with the mutual coherence function show very similar inversions in the same focus range around a calculated optimum of +3 nm (Fig. 3b). The plasmon-loss images, which carry only preserved elastic contrast, behave in the same way: within 6–8 nm of defocus their contrast also changes from dark to bright atoms and back (Fig. 4).

Why a single atom blurs
Simulations of a single isolated carbon atom showed where the core-loss contrast comes from (Fig. 5). In the plasmon-loss signal the atom can look brighter or darker than its surroundings, as in an elastic image. In the K-edge signal it always appears bright on a dark background with zero intensity. Away from the optimum focus, however, this bright spot spreads far beyond the 142 pm spacing of the carbon atoms in graphene, and at positive defocus it even becomes a ring that is stronger between the atoms than on them. Added up over the graphene lattice, these broad signals can also produce dark-atom images (Fig. 5b, bottom row).

Computing such an image is harder than for elastic scattering. An electron that loses energy leaves the atom in an excited state and becomes entangled with it, so the scattered electron can no longer be described by a single wave function, only by a mutual coherence function. For a single layer like graphene, the multislice calculation reduces to one slice in which elastic and inelastic scattering happen together. For the plasmon loss, ten partial waves describe the outgoing electron; the K-edge excitation needs thirty. Each of them travels through the lenses like an ordinary elastic wave, and the images for the single energy losses in the window are added up, weighted by the measured spectrum. The same code produced the simulated graphene focus series in Figs. 3b and 4b.

Both checks of the method, experiment against simulation and the averaging against a Fourier filter, are set out in the validation box below, which also shows how the averaging works (Figs. 6 and 7).

▸ Validation: experiment vs. simulation

The team was not the first to see this effect. Researchers at the Ernst Ruska Centre in Jülich had found it earlier with the chromatic and spherical aberration corrected FEI Titan PICO at 300 and 200 kV, in crystals tens of nanometers thick, and later also at 80 kV. Their simulations had raised the question that Ulm set out to answer: if elastic contrast dominates the core-loss image of a crystal tens of nanometers thick, would a single layer of light atoms finally give a clean elemental map? The comparison with graphene is set out in the next box.

▸ Validation: FEI Titan Themis SALVE at 80 kV vs. FEI Titan PICO at 80–300 kV

A scanning microscope at low voltage gives a second cross-check on the same material, graphene. Here the beam is focused to a probe and the energy-loss spectrum is recorded point by point, so the elastic phase contrast of the parallel beam plays a smaller role. The comparison with STEM-EELS at 60 kV is set out in the next box.

▸ Validation: FEI Titan Themis SALVE at 80 kV vs. Nion UltraSTEM at 60 kV

Challenges named by the authors
The core-loss signal needs a dose that destroys graphene within one to two minutes, so only a few single exposures could be recorded and every image had to be averaged over the lattice. The illumination was strongly condensed and uneven, and the automatic beam settings of the filter software did not compensate the beam tilt introduced at 300 eV offset, which can cause coma and astigmatism; the researchers re-centered the objective lens at that offset to limit it. A background subtraction with pre-edge windows was not possible because the signal just before the K edge was below the noise.

The image processing had to work around these limits. Hot and dead pixels were replaced by the median of their surroundings, and the strong intensity gradients of the uneven illumination were removed by subtracting a Gaussian-blurred copy of each image, much like a high-pass filter. Only small sub-regions with the best signal-to-noise ratio were cut from the 1024 × 1024 frames. The lattice used for the averaging came from the autocorrelation of a zero-loss image at the same magnification, and the results were cropped to the size of this kernel to avoid artifacts from the image borders.

A further limit lies in the physics itself. In the K-edge signal each carbon atom acts like a small, self-luminous point source, and such a source is imaged sharply only at the optimum focus. A few nanometers away from it, the signal of one atom already spreads wider than the 142 pm spacing in graphene, and true atomic resolution is lost. The result questions a widespread assumption, namely that chemical information can still be read directly from very thin samples in which multiple scattering is unlikely. In practice, the authors note, lattice-resolution EFTEM will not always give elemental maps with bright atoms. Two causes can act together: the ionization-edge signal itself can carry preserved elastic contrast, which is why the simulations reproduce the focus series only when they include elastic scattering, and the broad signal of each defocused atom adds up to dark atoms.

The findings, the authors conclude, “demonstrate the complications in atomic-resolution elemental mapping by EFTEM, even in Cc/Cs-corrected TEM.” Even for a single layer of light atoms, atomic-resolution core-loss images cannot be read directly as elemental maps, because preserved elastic contrast and the broad defocused signal of each atom can both turn bright atoms dark. For chemical mapping on the atomic scale, the authors point to alternatives: energy-filtered imaging scanning TEM, whose contrast stays stable even when the sample thickness changes[23],[24], and STEM-EELS, where elastic contributions are smaller, as shown for graphene[20]. The study, made with the chromatic and spherical aberration corrector of the SALVE microscope at Ulm University, shows where the limits of energy-filtered imaging lie.

Resource:
Mohn, M. J., Biskupek, J., Lee, Z., Rose, H., & Kaiser, U. (2020).
Lattice contrast in the core-loss EFTEM signal of graphene.
Ultramicroscopy 219, 113119.
https://doi.org/10.1016/j.ultramic.2020.113119

Download this news article as PDF – for reading on paper, taking notes or filing.

References
  1. Haider, M., Hartel, P., Müller, H., Uhlemann, S., Zach, J. (2010). Information Transfer in a TEM Corrected for Spherical and Chromatic Aberration. Microsc Microanal, 16, 393–408. https://doi.org/10.1017/S1431927610013498

  2. Kabius, B., Hartel, P., Haider, M., Muller, H., Uhlemann, S., Loebau, U., Zach, J., Rose, H. (2009). First Application of Cc-Corrected Imaging for High-Resolution and Energy-Filtered TEM. J. Electron Microsc., 58, 147–155. https://doi.org/10.1093/jmicro/dfp021

  3. Linck, M., Hartel, P., Uhlemann, S., Kahl, F., Müller, H., Zach, J., Haider, M., Niestadt, M., Bischoff, M., Biskupek, J., Lee, Z., Lehnert, T., Börrnert, F., Rose, H., Kaiser, U. (2016). Chromatic Aberration Correction for Atomic Resolution TEM Imaging From 20 to 80 kV. Phys. Rev. Lett., 117, 076101. https://doi.org/10.1103/PhysRevLett.117.076101

  4. SALVE news (2016). SALVE Cc Correction Realized. salve-project.de, August 9, 2016. https://salve-project.de/newspress/SALVE-CC-correction-realized.html

  5. Urban, K. W., Mayer, J., Jinschek, J. R., Neish, M. J., Lugg, N. R., Allen, L. J. (2013). Achromatic Elemental Mapping Beyond the Nanoscale in the Transmission Electron Microscope. Phys. Rev. Lett., 110, 185507. https://doi.org/10.1103/PhysRevLett.110.185507

  6. Forbes, B., Houben, L., Mayer, J., Dunin-Borkowski, R., Allen, L. (2014). Elemental Mapping in Achromatic Atomic-Resolution Energy-Filtered Transmission Electron Microscopy. Ultramicroscopy, 147, 98–105. https://doi.org/10.1016/j.ultramic.2014.07.002

  7. Rose, H. (1984). Information Transfer in Transmission Electron Microscopy. Ultramicroscopy, 15, 173–191. https://doi.org/10.1016/0304-3991(84)90038-X

  8. Howie, A. (1963). Inelastic Scattering of Electrons by Crystals. I. The theory of small-angle in elastic scattering. Proc. R. Soc. Lond. A, 271, 268–287. https://doi.org/10.1098/rspa.1963.0017

  9. Stallknecht, P., Kohl, H. (1996). Computation and Interpretation of Contrast in Crystal Lattice Images Formed by Inelastically Scattered Electrons in a Transmission Electron Microscope. Ultramicroscopy, 66, 261–275. https://doi.org/10.1016/S0304-3991(97)00007-7

  10. Navidi-Kasmai, T., Kohl, H. (2000). Computation of Contrasts in Atomic Resolution Electron Spectroscopic Images of Planar Defects in Crystalline Specimens. Ultramicroscopy, 81, 223–233. https://doi.org/10.1016/S0304-3991(99)00195-3

  11. Muller, D., Silcox, J. (1995). Delocalization in Inelastic Scattering. Ultramicroscopy, 59, 195–213. https://doi.org/10.1016/0304-3991(95)00029-Z

  12. Egerton, R. (2017). Scattering Delocalization and Radiation Damage in STEM-EELS. Ultramicroscopy, 180, 115–124. https://doi.org/10.1016/j.ultramic.2017.02.007

  13. Schattschneider, P., Nelhiebel, M., Jouffrey, B. (1999). Density Matrix of Inelastically Scattered Fast Electrons. Phys. Rev. B, 59, 10959–10969. https://doi.org/10.1103/PhysRevB.59.10959

  14. Müller, H., Rose, H., Schorsch, P. (1998). A Coherence Function Approach to Image Simulation. J. Microsc., 190, 73–88. https://doi.org/10.1046/j.1365-2818.1998.3050868.x

  15. Lee, Z., Hambach, R., Kaiser, U., Rose, H. (2017). Significance of Matrix Diagonalization in Modelling Inelastic Electron Scattering. Ultramicroscopy, 175, 58–66. https://doi.org/10.1016/j.ultramic.2016.11.011

  16. Lee, Z., Meyer, J., Rose, H., Kaiser, U. (2012). Optimum HRTEM Image Contrast at 20 kV and 80 kV—Exemplified by Graphene. Ultramicroscopy, 112, 39–46. https://doi.org/10.1016/j.ultramic.2011.10.009

  17. SALVE news (2012). Optimum HRTEM Contrast. salve-project.de, January 1, 2012. https://salve-project.de/newspress/optimum-hrtem-contrast.html

  18. Boothroyd, C. B., Moreno, M. S., Duchamp, M., Kovács, A., Monge, N., Morales, G. M., Barbero, C. A., Dunin-Borkowski, R. E. (2014). Atomic Resolution Imaging and Spectroscopy of Barium Atoms and Functional Groups on Graphene Oxide. Ultramicroscopy, 145, 66–73. https://doi.org/10.1016/j.ultramic.2014.03.004

  19. Dunin-Borkowski, R. E., Houben, L. (2016). Spherical and Chromatic Aberration Correction for Atomic-Resolution Liquid Cell Electron Microscopy. In F. M. Ross (Ed.), Liquid Cell Electron Microscopy (pp. 434–455). Cambridge University Press. https://doi.org/10.1017/9781316337455.022

  20. Kapetanakis, M. D., Zhou, W., Oxley, M. P., Lee, J., Prange, M. P., Pennycook, S. J., Idrobo, J. C., Pantelides, S. T. (2015). Low-Loss Electron Energy Loss Spectroscopy: An Atomic-Resolution Complement to Optical Spectroscopies and Application to Graphene. Phys. Rev. B, 92, 125147. https://doi.org/10.1103/PhysRevB.92.125147

  21. Gloter, A., Badjeck, V., Bocher, L., Brun, N., March, K., Marinova, M., Tencé, M., Walls, M., Zobelli, A., Stéphan, O., Colliex, C. (2017). Atomically Resolved Mapping of EELS Fine Structures. Mater. Sci. Semicond. Process., 65, 2–17. https://doi.org/10.1016/j.mssp.2016.07.006

  22. Bosman, M., Keast, V. J., García-Muñoz, J. L., D'Alfonso, A. J., Findlay, S. D., Allen, L. J. (2007). Two-Dimensional Mapping of Chemical Information at Atomic Resolution. Phys. Rev. Lett., 99, 086102. https://doi.org/10.1103/PhysRevLett.99.086102

  23. Brown, H., D'Alfonso, A., Forbes, B., Allen, L. (2016). Addressing Preservation of Elastic Contrast in Energy-Filtered Transmission Electron Microscopy. Ultramicroscopy, 160, 90–97. https://doi.org/10.1016/j.ultramic.2015.10.001

  24. Krause, F., Rosenauer, A., Barthel, J., Mayer, J., Urban, K., Dunin-Borkowski, R., Brown, H., Forbes, B., Allen, L. (2017). Atomic Resolution Elemental Mapping Using Energy-Filtered Imaging Scanning Transmission Electron Microscopy With Chromatic Aberration Correction. Ultramicroscopy, 181, 173–177. https://doi.org/10.1016/j.ultramic.2017.06.004