3D Electron Diffraction of MoS2

April 15, 2021 – Researchers at Ulm University have shown that three-dimensional electron diffraction tells the number of layers in freestanding MoS2 from one to five. Stacks with an odd number of layers have a mirror plane and give symmetric intensity along the reciprocal-lattice rods, stacks with an even number do not; together with the width of the peaks, this identifies each layer number. A flake counted optically as four layers turned out to have five.

How many layers does a flake of MoS2 have? For two-dimensional crystals the answer decides the properties: bulk MoS2 is a semiconductor with an indirect band gap, a single layer has a direct one[1]. Tatiana Gorelik, Berkin Nergis, Tobias Schöner, Janis Köster and Ute Kaiser at Ulm University have now shown that three-dimensional electron diffraction (3D ED) answers the question for freestanding MoS2 with one to five layers, directly in the transmission electron microscope. The key is symmetry. A single layer of MoS2 has a mirror plane in its middle; a bilayer loses it, because the second layer sits shifted against the first; a trilayer regains it (Fig. 1). In a tilt series of diffraction patterns this switch shows up plainly: for an odd number of layers the intensity along the reciprocal-lattice rods is symmetric, for an even number it is not. Together with the width of the intensity peaks, which shrinks as layers are added, it tells 1, 2, 3, 4 and 5 layers apart. A flake that had been counted as four layers before it went into the microscope turned out to have five.

Odd and even layers
Two-dimensional crystals are usually cut from layered bulk crystals, in which strong bonds within a layer meet weak van der Waals forces between layers, the strategy that began with graphene[2]. MoS2 is one of the best known. Its common bulk form, 2H-MoS2, has been known for almost a century: hexagonal layers with a lattice constant of 315 pm, each a sheet of molybdenum atoms sandwiched between two sheets of sulfur atoms, stacked with a repeat of 1230 pm along the c axis[3]. The unit cell holds two layers, the second shifted by a third of the cell diagonal against the first (AB stacking), and the bulk crystal is centrosymmetric.

A crystal that is periodic in only two directions is described by a layer group[4]. A single layer of 2H-MoS2 has a horizontal mirror plane through its molybdenum sheet and a vertical six-fold rotoinversion axis; its layer group is p-6m2 (No. 78). In a bilayer the shift between the layers destroys the horizontal mirror plane, and the axis becomes a three-fold one: the layer group is p-3m1 (No. 72). A trilayer regains the mirror plane, a four-layer crystal loses it again. Every stack with an odd number of layers therefore has the higher symmetry p-6m2, every stack with an even number the lower symmetry p-3m1. In diffraction, the higher symmetry includes a horizontal mirror plane in reciprocal space, so the intensity along each rod must be symmetric about its base; the lower symmetry lacks it, and the intensity may be asymmetric.

Rods instead of spots
3D electron diffraction collects diffraction patterns while the sample is tilted step by step and reassembles them into a three-dimensional map of reciprocal space. Developed for the structure analysis of nanocrystals[5], it had recently been used to tell graphene stacks apart[6]. For a crystal only a few atoms thick, the diffraction spots of a bulk crystal stretch into continuous rods, the relrods, running perpendicular to the layers (Fig. 2). The coordinate along a rod, L, is no longer an integer index but continuous, and the rod’s profile holds the information on the structure across the layers. In the reconstruction of a single layer the rods appear long and smooth; their cuts show how much intensity each one carries along its length (Fig. 3).

The team tilted each flake from −60° to +60° in steps of 1° and extracted the intensity along three kinds of rods, labelled 10-1L, 11-2L and 20-2L by the reflections they pass through at L = 0. Standard crystallographic programs cannot calculate the continuous intensity of a confined crystal, so the team built artificial crystals with one to five layers in a cell 100 nm high and calculated their diffraction in the kinematic approximation. The simulated rods show the alternation at a glance: symmetric for one, three and five layers, asymmetric for two and four, with peaks that grow narrower and approach the Bragg reflections of the bulk crystal. How the simulations were set up is described in the box below.

▸ How the simulation works

One layer to five
For a monolayer, the measured profiles of all three rod types agree well with the simulation, including the widths of the peaks (Table 1). Equivalent rods give practically the same profile, so the peak width comes from the atomic scattering factors, not from the instrument. Only in the middle of the 10-1L rods do the two Friedel mates, the reflections on opposite sides of the pattern, differ by about 20 %. A kinematic calculation cannot give this: in a crystal without inversion centre that contains heavy atoms, the scattering breaks Friedel’s law, an effect earlier seen in single-layer MoS2[8] and explained by strong phase-object scattering[9]. How Ulm’s observation compares with a 4D-STEM study at Cornell is shown in a box further below.

The bilayer shows the predicted asymmetry, measured and simulated alike (Table 1). Of two neighbouring 10-1L rods, one has its peak at L = +1.6 nm−1, the other at −1.6 nm−1, exactly as calculated, and the 20-2L rods are asymmetric at the same height. Small peak shifts at larger L, mainly in the 11-2L rods, may point to an atomic arrangement slightly different from the bulk.

The trilayer is symmetric about the rod base, the four-layer crystal clearly asymmetric between 0 and 2 nm−1, and the five-layer crystal symmetric again. Table 1 sums up the measured profiles for each layer number. The five-layer crystal was a surprise. Both crystals had been chosen as four-layer flakes by their optical contrast, but the second showed a completely different pattern: symmetric rods with peaks as narrow as those of four layers. The symmetry assigned it unambiguously to five layers.

LayersLayer groupRods about L = 0Simulated 10-1L rodMeasured vs. simulatedPeak width (10-1L, L = 2.2 nm−1)
1p-6m2 (No. 78)symmetricbroad peaks; strongest at 3.15 nm−1 (S–S distance)all three rod types agree, peak widths too; Friedel mates differ by ≈ 20 % at L = 0≈ 2.1 nm−1
2p-3m1 (No. 72)asymmetricshoulder at 1.62 nm−1 on one side only (Mo–Mo, 615 pm)10-1L peaks at +1.6 and −1.6 nm−1 on neighbouring rods, 20-2L asymmetric at the same height, as calculated; 11-2L peaks slightly shifted at larger L≈ 0.7 nm−1
3p-6m2symmetricfirst weak peak at 0.81 nm−1 (c = 1230 pm)symmetric about the rod base, as calculated≈ 0.6 nm−1
4p-3m1asymmetricnarrower peaks, approaching bulkclearly asymmetric between 0 and 2 nm−1≈ 0.4 nm−1
5p-6m2symmetricclose to the bulk Bragg peakssymmetric; flake counted optically as four layers≈ 0.4 nm−1

Table 1: Layer number of MoS₂ from 3D ED: symmetry, rod profiles and peak width (this work).

The width of the peaks is the second fingerprint. Measured on the 10-1L rod at L = 2.2 nm−1, it drops from about 2.1 nm−1 for one layer to 0.7 for two, 0.6 for three and 0.4 nm−1 for four and five layers (Table 1). The width alone separates the monolayer clearly, but it levels off for thicker crystals; there, the symmetry decides between odd and even. Together, width and symmetry give the layer number unambiguously. The analysis also showed that the decisive differences lie at L below 2 nm−1. Sampling the 10-1L rod between −1.6 and +1.6 nm−1 would be enough, and since the rod stands 3.7 nm−1 from the centre, a tilt range of ±30° would do instead of ±60°.

Measured at 300 kV, a bilayer shows its asymmetry only when it is tilted. At lower voltage the curved Ewald sphere cuts the rods higher up, so even an untilted pattern should reveal a bilayer. The box below estimates how strong the effect is at the voltages of a low-voltage microscope (Fig. 4).

▸ Low voltage: a bilayer without tilting

Before the flakes went into the microscope, their thickness had been estimated by optical contrast against published reference values from Nanyang Technological University in Singapore[10]. How the two methods compare is shown in the box below.

▸ Validation: 3D ED vs. optical contrast

The Friedel asymmetry in the monolayer, finally, has an independent counterpart: a 4D-STEM study at Cornell University measured the same effect in single-layer MoS2 and explained it, as summarized in the box below.

▸ Validation: Titan TEM at 300 kV vs. Titan Themis 4D-STEM at 60 kV

From rods to rings: the electron PDF
3D ED needs a single crystal, even if it is only one layer thick. For materials without long-range order, such as glasses, amorphous films and nanoparticles a few nanometers across, the same group uses the powder pattern instead. Two years earlier, Tatiana Gorelik, Ute Kaiser and partners from Erlangen, Stuttgart and Karlsruhe had reviewed how such patterns are turned into a pair distribution function (PDF), a histogram of all interatomic distances in the sample, and how far an electron PDF (ePDF) can be refined quantitatively[7]. In gold particles of 4, 8 and 20 nm, the PDF peaks die out at 1.5, 3 and more than 5 nm, and in anatase (TiO2) crystals 5 nm in size, energy filtering hardly changed the PDF, because inelastic scattering mostly adds a smooth background[7]. Refined in three programs, the electron data gave the same anatase structure as synchrotron X-rays, with lattice parameters about 1.5 % larger, a camera-length error typical of electron diffraction[7].

As for the bilayer asymmetry above, the voltage matters: the lower it is, the shorter the distance an electron travels before it scatters, and the thinner a sample must be. The box below gives the numbers (Fig. 5).

▸ Mean free path from 20 to 300 kV

How reliable lattice parameters from an ePDF are had been tested at Brookhaven National Laboratory with a different microscope, as the box below shows.

▸ Validation: FEI Titan at 300 kV vs. JEOL ARM 200CF at 200 kV

Microscope, sample preparation and software are listed in the box below.

▸ Instruments and samples

Challenges named by the authors
The analysis was qualitative. Fine differences between simulated and measured profiles remain, and the authors name three causes: the structure of few-layer MoS2 may differ slightly from the bulk structure the models were built from; multiple scattering is evidently present in the data, while the simulation is kinematic; and the instrumental transfer function in diffraction space has not yet been seriously addressed. A slight difference between the left and right peaks of the monolayer at 3 nm−1 is still open, whether it also comes from anomalous scattering or from the measurement. Single-layer MoS2 is corrugated, like graphene[14], and the ripples broaden the rods at larger L[8]; since the rod profile is itself complex, quantifying the corrugation may need a more sophisticated formalism, and the study did not attempt it.

Outlook
3D electron diffraction identifies the number of layers in MoS2 from one to five on the freestanding flake, from two features: the symmetry of the rods, which separates odd from even, and the width of their peaks. A tilt range of ±30° is enough. Since the alternation of symmetry follows from the AB stacking alone, the method should carry over to other transition metal dichalcogenides with the same structure. At low voltage the curved Ewald sphere may even reveal a bilayer in a single untilted pattern. The work was funded by the DFG through the collaborative research centre CRC 1279 and by the European Union through the Graphene Flagship.

Resource:
Gorelik, T. E., Nergis, B., Schöner, T., Köster, J., & Kaiser, U. (2021).
3D electron diffraction of mono- and few-layer MoS2.
Micron 146, 103071.
https://doi.org/10.1016/j.micron.2021.103071

Update – June 1, 2022

The news article of April 15, 2021 ends above. Later work that builds on it is listed below.

3D ED among the TEM methods
Janis Köster, Tatiana Gorelik, Ute Kaiser and colleagues compared high-resolution TEM, electron energy-loss spectroscopy and 3D electron diffraction for counting the layers of freestanding MoS2 and MoTe2 with one to four layers[15]. HRTEM reliably singles out the monolayer, while momentum-resolved EELS and 3D ED distinguish up to four layers; diffraction proved the least affected by contamination and the gentlest on the sample (see TEM Layer Identification MoS2/MoTe2[16]).

Download this news article as PDF – for reading on paper, taking notes or filing.

References
  1. Mak, K. F., Lee, C., Hone, J., Shan, J., Heinz, T. F. (2010). Atomically Thin MoS2: A New Direct-Gap Semiconductor. Phys. Rev. Lett., 105, 136805. https://doi.org/10.1103/PhysRevLett.105.136805

  2. Xu, M., Liang, T., Shi, M., Chen, H. (2013). Graphene-Like Two-Dimensional Materials. Chem. Rev., 113, 3766–3798. https://doi.org/10.1021/cr300263a

  3. Dickinson, R. G., Pauling, L. (1923). The Crystal Structure of Molybdenite. J. Am. Chem. Soc., 45, 1466–1471. https://doi.org/10.1021/ja01659a020

  4. Kopský, V., Litvin, D. B. (Eds.) (2002). International Tables for Crystallography, Volume E: Subperiodic Groups. Dordrecht: Kluwer.

  5. Gemmi, M., Mugnaioli, E., Gorelik, T. E., Kolb, U., Palatinus, L., Boullay, P., Hovmöller, S., Abrahams, J. P. (2019). 3D Electron Diffraction: The Nanocrystallography Revolution. ACS Cent. Sci., 5, 1315–1329. https://doi.org/10.1021/acscentsci.9b00394

  6. Sung, S. H., Schnitzer, N., Brown, L., Park, J., Hovden, R. (2019). Stacking, Strain, and Twist in 2D Materials Quantified by 3D Electron Diffraction. Phys. Rev. Mater., 3, 064003. https://doi.org/10.1103/PhysRevMaterials.3.064003

  7. Gorelik, T. E., Neder, R., Terban, M. W., Lee, Z., Mu, X., Jung, C., Jacob, T., Kaiser, U. (2019). Towards Quantitative Treatment of Electron Pair Distribution Function. Acta Cryst. B, 75, 532–549. https://doi.org/10.1107/S205252061900670X

  8. Brivio, J., Alexander, D. T. L., Kis, A. (2011). Ripples and Layers in Ultrathin MoS2 Membranes. Nano Lett., 11, 5148–5153. https://doi.org/10.1021/nl2022288

  9. Deb, P., Cao, M. C., Han, Y., Holtz, M. E., Xie, S., Park, J., Hovden, R., Muller, D. A. (2020). Imaging Polarity in Two Dimensional Materials by Breaking Friedel’s Law. Ultramicroscopy, 215, 113019. https://doi.org/10.1016/j.ultramic.2020.113019

  10. Li, H., Wu, J., Huang, X., Lu, G., Yang, J., Lu, X., Xiong, Q., Zhang, H. (2013). Rapid and Reliable Thickness Identification of Two-Dimensional Nanosheets Using Optical Microscopy. ACS Nano, 7, 10344–10353. https://doi.org/10.1021/nn4047474

  11. Abeykoon, A. M. M., Hu, H., Wu, L., Zhu, Y., Billinge, S. J. L. (2015). Calibration and Data Collection Protocols for Reliable Lattice Parameter Values in Electron Pair Distribution Function Studies. J. Appl. Cryst., 48, 244–251. https://doi.org/10.1107/S1600576715000412

  12. Das, S., Robinson, J. A., Dubey, M., Terrones, H., Terrones, M. (2015). Beyond graphene: progress in novel two-dimensional materials and van der Waals solids. Annu. Rev. Mater. Res., 45, 1–27. https://doi.org/10.1146/annurev-matsci-070214-021034

  13. Lehnert, T., Lehtinen, O., Algara-Siller, G., Kaiser, U. (2017). Electron Radiation Damage Mechanisms in 2D MoSe2. Appl. Phys. Lett., 110, 033106. https://doi.org/10.1063/1.4973809

  14. Meyer, J. C., Geim, A. K., Katsnelson, M. I., Novoselov, K. S., Booth, T. J., Roth, S. (2007). The Structure of Suspended Graphene Sheets. Nature, 446, 60–63. https://doi.org/10.1038/nature05545

  15. Köster, J., Storm, A., Gorelik, T. E., Mohn, M. J., Port, F., Gonçalves, M. R., Kaiser, U. (2022). Evaluation of TEM Methods for Their Signature of the Number of Layers in Mono- and Few-Layer TMDs as Exemplified by MoS2 and MoTe2. Micron, 160, 103303. https://doi.org/10.1016/j.micron.2022.103303

  16. SALVE news (2022). TEM Layer Identification MoS2/MoTe2. salve-project.de, June 1, 2022. https://www.salve-project.de/newspress/tem_layer_identification_mos2_mote2.html